📏 Vickers hardness testing machines — direct verification (test force, 136° diamond indenter, diagonal measuring system, testing cycle) and indirect verification on reference blocks according to ISO 6507-3: five indentations, repeatability and bias; PN-EN ISO 6507-2
In short
Verification and calibration of testing machines for Vickers hardness testing according to ISO 6507-1, including portable machines, by the direct and the indirect method. The test is performed according to PN-EN ISO 6507-2:2018-05 (English version; implements EN ISO 6507-2:2018 and ISO 6507-2:2018 [IDT]); STATUS (PKN card, 15.11.2026): PN-EN ISO 6507-2:2018-05 (English version, published 04-05-2018); implements EN ISO 6507-2:2018 and ISO 6507-2:2018; replaces PN-EN ISO 6507-2:2007. The procedure comprises 6 steps; it is used for: Vickers hardness testing machines, including portable ones — verification before first use, after repair and periodically (ISO 6507-2:2018, clauses 1 and 7), Each test force used in testing — blocks calibrated with the same force (6.2), Not for machines based on a different principle, e.g. the ultrasonic impedance method (clause 1).
At a glance
- Standard: PN-EN ISO 6507-2:2018-05 (English version; implements EN ISO 6507-2:2018 and ISO 6507-2:2018 [IDT])
- Category: Metrology
- Procedure steps: 6
- STATUS (PKN card, 15.11.2026): PN-EN ISO 6507-2:2018-05 (English version, published 04-05-2018); implements EN ISO 6507-2:2018 and ISO 6507-2:2018; replaces PN-EN ISO 6507-2:2007
- Temperature (5.1.3, 6.1.3): (23 ± 5) °C; outside this range — stated in the report
- Test force (5.2, table 1): 3 readings at each position; ±2,0 % (0,009 807 N to < 0,098 07 N), ±1,5 % (to < 1,961 N), ±1,0 % (≥ 1,961 N)
Overview
WHAT THE STANDARD COVERS. According to clause 1 of ISO 6507-2:2018 the document specifies a method of verification and calibration of testing machines and of the diagonal measuring system for determining Vickers hardness in accordance with ISO 6507-1. The direct method concerns the testing machine, the indenter and the diagonal length measuring system, and the indirect method — the overall check of the machine on reference blocks. A machine also used for other hardness test methods is verified independently for each method. The document also applies to portable machines, but not to machines based on a different principle, e.g. the ultrasonic impedance method. The PKN card of PN-EN ISO 6507-2:2018-05 gives the same scope.
ACCORDING TO THE TEXT OF ISO 6507-2:2018 (publisher's sample in English: foreword, clauses 1–7 and the beginning of clause 8). The standard was prepared by ISO/TC 164 (Mechanical testing of metals), subcommittee SC 3 (Hardness testing); the fourth edition replaced the third (ISO 6507-2:2005) after technical revision — all references to indentation diagonals smaller than 0,020 mm were removed, the requirements for calibration and verification of the measuring system and the maximum permissible error in measuring a reference indentation were changed, recommendations for inspection of the indenter were moved to ISO 6507-1, the hardness of the reference blocks used was added to the report, annex A was revised. Normative references: ISO 376, ISO 6507-1 and ISO 6507-3. General conditions (clause 4): before verification the machine is set up according to the manufacturer's instructions — the plunger holding the indenter slides in its guide without friction or excessive side play, the indenter holder is firmly mounted, the force is applied and removed without shock, vibration or overshoot, and in the diagonal measuring system the change to measuring mode does not influence the reading, the illumination is uniform and gives contrast at the edge of the indentation. Note to clause 4: the tolerances of the standard already include the uncertainty of the instruments and reference standards, so they are not further reduced by the measurement uncertainty. Direct verification (clause 5) is recommended at (23 ± 5) °C — outside this range this is stated in the report — with instruments traceable to national standards. Test forces (5.2): each force within the working range is measured, and when the indenter position affects the force — at not less than three plunger positions (with a closed-loop system one is enough); with an instrument according to ISO 376 class 1 or better or by balancing against a force accurate to ±0,2 %; the output of the instrument should not vary by more than 0,2 % within 1 s to 30 s after a stepped change in force; three readings of each force at each position. Permissible relative error ΔF_rel (table 1): 0,009 807 N ≤ F < 0,098 07 N — ±2,0 %; 0,098 07 N ≤ F < 1,961 N — ±1,5 %; F ≥ 1,961 N — ±1,0 %. Indenter (5.3): the four faces of the diamond pyramid polished and free from defects; the shape is verified by direct or optical measurement with a device of maximum expanded uncertainty 0,07°; angle between opposite faces 136° ± 0,5° (or between opposite edges 148,11° ± 0,76°); angle between the pyramid axis and the holder axis less than 0,5°; maximum permissible length of the line of junction between opposite faces (table 2): 0,000 5 mm for 0,009 807 N ≤ F < 1,961 N, 0,001 mm for 1,961 N ≤ F < 49,03 N, 0,002 mm for F ≥ 49,03 N; the indenter shall have a valid calibration certificate. Diagonal measuring system (5.4): verified at each magnification and for each scale, in both perpendicular orientations, on a calibrated stage micrometer (expanded uncertainty of the line intervals not greater than 0,000 4 mm or 0,2 % — whichever is greater); at least four evenly spaced intervals in the centre of the field of view, three measurements each, each with an error not greater than 0,000 8 mm or 1,0 % of the measured length (whichever is greater). The testing cycle (5.5) is timed with equipment of maximum expanded uncertainty 1 s; the times shall be within the limits of ISO 6507-1. Uncertainty of the results — example in annex A (5.6).
INDIRECT VERIFICATION (clause 6) is recommended at (23 ± 5) °C on reference blocks calibrated according to ISO 6507-3 with the same forces that the machine will use. When verifying several forces — for each force at least two blocks from the ranges < 250 HV, 400 HV to 600 HV, > 700 HV, the whole set including at least one block from each range; with one force — three blocks, one from each range. On each block one of the reference indentations from the current calibration period is measured — difference of the mean from the certified mean diagonal length not greater than 0,001 mm or 1,25 % (whichever is greater). Five indentations are made and measured on each block according to ISO 6507-1, on the calibrated surface only. Repeatability: r_rel = 100 × (H₅ − H₁)/H̄; it is satisfactory when d₁ − d₅ ≤ 0,001 mm, otherwise when r_rel does not exceed table 4 — for blocks ≤ 250 HV: 6,0 % (HV 5 to HV 100), 12,0 % (HV 0,2 to < HV 5), 18,0 % (< HV 0,2); for blocks > 250 HV: 4,0 %, 8,0 % and 12,0 %. Bias: b = H̄ − H_CRM, b_rel = 100 × (H̄ − H_CRM)/H_CRM, where H_CRM is the certified hardness of the block; permissible b_rel (table 5): ±(0,21/d̄ + 1,5) % for 0,02 mm ≤ d̄ < 0,14 mm and ±3 % for 0,14 mm ≤ d̄ ≤ 1,4 mm. Uncertainty — annex A (6.8).
INTERVALS (clause 7). Indirect verification at least once every 12 months and after each direct verification; direct verification is recommended every 12 months and is performed according to table 6: before first use — force, diagonal measuring system, cycle and indenter; after dismantling and reassembling if the force, diagonal measuring system or cycle are affected, after failure of indirect verification and when the last indirect verification was more than 13 months ago — force, diagonal measuring system and cycle; it is recommended that the indenter be directly verified after 2 years of use. After a failed indirect verification the parameters may be verified sequentially, and direct verification is not required if it is shown (e.g. with a reference indenter) that the indenter was the cause. The report / certificate (8.1) gives, among other things, reference to ISO 6507-2, the method of verification (direct or indirect) and identification data of the machine; the sample does not include the further items of clause 8 or annex A.
STATUS (PKN card, read 15.11.2026). PN-EN ISO 6507-2:2018-05 — English version, Polish title “Metale -- Pomiar twardości sposobem Vickersa -- Część 2: Sprawdzanie i wzorcowanie twardościomierzy”, published 04-05-2018, 30 pages, KT 123 for Testing of Properties of Metals, implements EN ISO 6507-2:2018 and ISO 6507-2:2018 [IDT], replaces PN-EN ISO 6507-2:2007 (Polish version); the card gives no withdrawal date. iTeh catalogue (15.11.2026): ISO 6507-2:2018 — published 10.01.2018, stage “International Standard confirmed” (90.93).
IN ACCREDITATION SCOPES (scope database of the service, read 15.11.2026, after loading the scopes of this batch). PN-EN ISO 6507-2 appears at 9 Polish calibration laboratories (1 record each) — usually in the 2018-05 edition, at four alongside ASTM E92-23 and ASTM E384-22, at two as the basis of an internal procedure — and at 3 Czech laboratories.
Method principle
The machine is verified in two ways. Directly — by measuring the test forces with an instrument according to ISO 376 class 1 or better (error ±1,0 % to ±2,0 % depending on the force), the indenter geometry (136° ± 0,5°, line of junction according to table 2), the diagonal measuring system on a stage micrometer and the testing cycle. Indirectly — by making five indentations on reference blocks calibrated according to ISO 6507-3 from the ranges < 250 HV, 400 HV to 600 HV and > 700 HV and comparing the repeatability r_rel and the bias b_rel with tables 4 and 5.
Applications
- Vickers hardness testing machines, including portable ones — verification before first use, after repair and periodically (ISO 6507-2:2018, clauses 1 and 7)
- Each test force used in testing — blocks calibrated with the same force (6.2)
- Not for machines based on a different principle, e.g. the ultrasonic impedance method (clause 1)
- In accreditation scopes: 9 Polish calibration laboratories and 3 Czech
Key parameters
| Parameter | Value |
|---|---|
| STATUS (PKN card, 15.11.2026) | PN-EN ISO 6507-2:2018-05 (English version, published 04-05-2018); implements EN ISO 6507-2:2018 and ISO 6507-2:2018; replaces PN-EN ISO 6507-2:2007 |
| Temperature (5.1.3, 6.1.3) | (23 ± 5) °C; outside this range — stated in the report |
| Test force (5.2, table 1) | 3 readings at each position; ±2,0 % (0,009 807 N to < 0,098 07 N), ±1,5 % (to < 1,961 N), ±1,0 % (≥ 1,961 N) |
| Indenter (5.3) | 136° ± 0,5° between faces (148,11° ± 0,76° between edges); axis < 0,5°; line of junction 0,000 5 / 0,001 / 0,002 mm (table 2) |
| Diagonal measuring system (5.4, table 3) | stage micrometer: 0,000 4 mm or 0,2 %; ≥ 4 intervals × 3 measurements; error ≤ 0,000 8 mm or 1,0 % |
| Cycle (5.5) | timing equipment of expanded uncertainty ≤ 1 s; limits of ISO 6507-1 |
| Blocks (6.2) | ranges < 250 HV, 400 HV to 600 HV, > 700 HV; ≥ 2 blocks per force; with one force — 3 blocks; 5 indentations per block |
| Reference indentation (6.3) | difference from the certified diagonal ≤ 0,001 mm or 1,25 % |
| Repeatability r_rel (table 4) | ≤ 250 HV: 6,0 / 12,0 / 18,0 %; > 250 HV: 4,0 / 8,0 / 12,0 % (HV 5–HV 100 / HV 0,2–< HV 5 / < HV 0,2); d₁ − d₅ ≤ 0,001 mm is sufficient |
| Bias b_rel (table 5) | ±(0,21/d̄ + 1,5) % for 0,02 mm ≤ d̄ < 0,14 mm; ±3 % for 0,14 mm ≤ d̄ ≤ 1,4 mm |
| Intervals (clause 7, table 6) | indirect ≥ once every 12 months and after direct; direct recommended every 12 months; indenter after 2 years |
| Coverage in accreditation scopes (read 15.11.2026) | 9 Polish calibration laboratories (9 records); 3 Czech |
Standard
- Standard number
- PN-EN ISO 6507-2:2018-05 (English version; implements EN ISO 6507-2:2018 and ISO 6507-2:2018 [IDT])
- Title (PL)
- Metale — Pomiar twardości sposobem Vickersa — Część 2: Sprawdzanie i wzorcowanie twardościomierzy
- Title (EN)
- Metallic materials — Vickers hardness test — Part 2: Verification and calibration of testing machines
Step-by-step procedure
-
General conditions
Check of the set-up according to the manufacturer's instructions: plunger guide, mounting of the indenter holder, application of the force without shock, illumination and change to diagonal measurement (clause 4).
-
Test forces
Three readings of each force at each plunger position; relative error within the limits of table 1 (5.2).
-
Indenter
Faces, angle 136° ± 0,5°, inclination of the axis, line of junction against table 2; valid calibration certificate (5.3).
-
Diagonal measuring system and cycle
Each magnification and scale, both orientations; at least four stage micrometer intervals with three measurements each; cycle times within the limits of ISO 6507-1 (5.4–5.5).
-
Indirect verification
Selection of blocks from three hardness ranges, measurement of the reference indentation, five indentations each; r_rel and b_rel against tables 4 and 5 (clause 6).
-
Intervals and report
Dates according to clause 7 and table 6; report with reference to ISO 6507-2, the method of verification and the machine data (8.1).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Force-measuring instrument (5.2.2) | According to ISO 376, class 1 or better; or balancing against a force accurate to ±0,2 % (calibrated masses) | — |
| Device for verifying the indenter shape (5.3.2) | Direct or optical measurement, expanded uncertainty ≤ 0,07° | — |
| Stage micrometer (5.4) | Calibrated; expanded uncertainty of the line intervals ≤ 0,000 4 mm or 0,2 % | — |
| Reference blocks (6.2) | Calibrated according to ISO 6507-3 with the same forces, with certified hardness H_CRM and reference indentations | — |
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN ISO 6507-2:2018-05 (English version; implements EN ISO 6507-2:2018 and ISO 6507-2:2018 [IDT]) — “Metallic materials — Vickers hardness test — Part 2: Verification and calibration of testing machines”.
How does this method work?
The machine is verified in two ways. Directly — by measuring the test forces with an instrument according to ISO 376 class 1 or better (error ±1,0 % to ±2,0 % depending on the force), the indenter geometry (136° ± 0,5°, line of junction according to table 2), the diagonal measuring system on a stage micrometer and the testing cycle.
What is the measuring range and accuracy?
STATUS (PKN card, 15.11.2026): PN-EN ISO 6507-2:2018-05 (English version, published 04-05-2018); implements EN ISO 6507-2:2018 and ISO 6507-2:2018; replaces PN-EN ISO 6507-2:2007; Temperature (5.1.3, 6.1.3): (23 ± 5) °C; outside this range — stated in the report; Test force (5.2, table 1): 3 readings at each position; ±2,0 % (0,009 807 N to < 0,098 07 N), ±1,5 % (to < 1,961 N), ±1,0 % (≥ 1,961 N); Indenter (5.3): 136° ± 0,5° between faces (148,11° ± 0,76° between edges); axis < 0,5°; line of junction 0,000 5 / 0,001 / 0,002 mm (table 2).
How long does the test take?
The procedure comprises 6 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.
What equipment is required?
Force-measuring instrument (5.2.2), Device for verifying the indenter shape (5.3.2), Stage micrometer (5.4), Reference blocks (6.2).
Where is this test used?
Vickers hardness testing machines, including portable ones — verification before first use, after repair and periodically (ISO 6507-2:2018, clauses 1 and 7); Each test force used in testing — blocks calibrated with the same force (6.2); Not for machines based on a different principle, e.g. the ultrasonic impedance method (clause 1); In accreditation scopes: 9 Polish calibration laboratories and 3 Czech.
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 6507-2.