📏 Brinell hardness testing machines — direct verification (test force, ball, indentation diameter measuring system, testing cycle) and indirect verification on reference blocks according to ISO 6506-3: five indentations, repeatability and error of the machine; PN-EN ISO 6506-2
In short
Verification of testing machines for Brinell hardness testing according to ISO 6506-1, stationary and portable, by the direct and the indirect method. The test is performed according to PN-EN ISO 6506-2:2019-10 (English version; implements EN ISO 6506-2:2018 and ISO 6506-2:2017 [IDT]); STATUS (PKN card, 15.11.2026): PN-EN ISO 6506-2:2019-10 (English version, published 29-10-2019); implements EN ISO 6506-2:2018 and ISO 6506-2:2017; replaces PN-EN ISO 6506-2:2014-12. The procedure comprises 6 steps; it is used for: Brinell hardness testing machines, stationary and portable — verification before first use, after repair and periodically (ISO 6506-2:2017, clauses 1 and 7), Each test force and each ball diameter used in testing (6.2), Machines that cannot meet the force–time profile — modified verification of force and cycle according to annex B (clause 1).
At a glance
- Standard: PN-EN ISO 6506-2:2019-10 (English version; implements EN ISO 6506-2:2018 and ISO 6506-2:2017 [IDT])
- Category: Metrology
- Procedure steps: 6
- STATUS (PKN card, 15.11.2026): PN-EN ISO 6506-2:2019-10 (English version, published 29-10-2019); implements EN ISO 6506-2:2018 and ISO 6506-2:2017; replaces PN-EN ISO 6506-2:2014-12
- Temperature (5.1.1, 6.1): (23 ± 5) °C; outside this range — stated in the report
- Test force (5.2): 3 readings of each force, with a lever at ≥ 3 indenter positions; instrument ISO 376 cl. 1 or masses ±0,2 %; each reading ±1,0 % of the nominal force
Overview
WHAT THE STANDARD COVERS. According to clause 1 of ISO 6506-2:2017 the document specifies methods of direct and indirect verification of testing machines used for Brinell hardness testing in accordance with ISO 6506-1, and when these two types of verification are to be performed. Direct verification checks whether individual parameters of the machine are within specified limits, and indirect verification uses hardness measurements on reference blocks calibrated according to ISO 6506-3 to check the performance of the machine as a whole. A machine also used for other hardness test methods is verified independently for each method. The document applies to stationary and portable testing machines; for machines that cannot meet the required force–time profile, direct verification of the force and the testing cycle may be modified according to annex B. The PKN card of PN-EN ISO 6506-2:2019-10 gives the same scope.
ACCORDING TO THE TEXT OF ISO 6506-2:2017 (publisher's sample in English: foreword, clauses 1–8). The standard was prepared by ISO/TC 164 (Mechanical testing of metals), subcommittee SC 3 (Hardness testing); the fourth edition replaced the third (ISO 6506-2:2014) after technical revision — clause 3 was added and table 3 changed. Normative references: ISO 376, ISO 6506-1:2014, ISO 6506-3 and ISO 6507-1. General conditions (clause 4): before verification the machine is set up according to the manufacturer's instructions; in particular the ball-holder plunger slides correctly in its guide, each ball holder is firmly mounted, the force is applied and removed without shock, vibration or overshoot, and with an integral diameter measuring system the change to measuring mode and the illumination do not affect the result. Direct verification (clause 5) is recommended at (23 ± 5) °C — outside this range this is stated in the report — with instruments traceable to SI. Test forces (5.2): each force is measured within the working range; with a lever-applied force in an open-loop system — at not less than three positions of the indenter uniformly spaced over its travel; three readings of each force at each position, the indenter being moved in the same direction as in testing before each reading; measurement with an instrument according to ISO 376 class 1 or better or by balancing against a force accurate to ±0,2 % (calibrated masses); each reading within ±1,0 % of the nominal test force. Ball (5.3): only the ball is verified; at least two balls are selected at random from a batch, each checked for size and hardness and then discarded; balls polished and free from defects; diameter — the mean of at least three measurements at different positions, none deviating from the nominal by more than the tolerance of table 1 (10 mm: ±0,005 mm; 5 mm: ±0,004 mm; 2,5 mm: ±0,003 mm; 1 mm: ±0,003 mm); hardmetal balls: hardness at least 1 500 HV according to ISO 6507-1, density (14,8 ± 0,2) g/cm³; recommended composition: tungsten carbide — balance, total other carbides 2,0 %, cobalt 5,0 % to 7,0 %; the user measures the balls or buys them from a supplier certifying compliance. Indentation diameter measuring system (5.4): with direct measurement the scale shall allow the diameter to be estimated within ±0,5 %; calibration for each objective and each scale, in two perpendicular axes, on a stage micrometer at not less than four intervals in the centre of the field of view, difference ≤ 0,5 %; with the diameter calculated from the projected area — at least four reference circular images, error ≤ 1 % of the area; every system is also checked on certified reference indentations (e.g. on blocks according to ISO 6506-3) — at least four indentations for each ball diameter and each objective, mean within 0,5 % of the certified diameter. The testing cycle (5.5) is verified by the manufacturer at manufacture and after a repair that may have affected it, otherwise according to table 4; the cycle shall conform to ISO 6506-1 taking into account the uncertainty of the time measurement.
INDIRECT VERIFICATION (clause 6) is recommended at (23 ± 5) °C on reference blocks calibrated according to ISO 6506-3; the surfaces of the blocks and indenters free from additives and corrosion products. The machine is verified for each force and each ball diameter — for each force at least two blocks from the hardness ranges of table 2 (force–diameter ratio 0,102 × F/D² = 30) or table 3 (other ratios), where possible from different ranges. If indirect verification does not immediately follow direct verification, a reference indentation on each block is measured with the same illumination as at the last direct verification — difference ≤ 0,5 % of the certified diameter. Five indentations uniformly distributed over the surface are made on each block. Repeatability: r = d₅ − d₁, relative r_rel = 100 × (d₅ − d₁)/d̄; error: E = H̄ − H_C, relative E_rel = 100 × (H̄ − H_C)/H_C, where H_C is the certified hardness of the block. Permissible values (table 2, ratio 30): H_C < 250 HBW — r_rel 3,0 %, E_rel ±3,0 %; 250 HBW to 450 HBW — 2,5 % and ±2,5 %; > 450 HBW — 2,0 % and ±2,0 %; table 3 (ratios 15, 10, 5, ≤ 2,5) — 3,0 % and ±3,0 % in all ranges. Uncertainty of the results — annex A.
INTERVALS AND REPORT (clauses 7–8). Indirect verification at least once every 12 months and after each direct verification. Direct verification (table 4): before first use — force, diameter measuring system, testing cycle and indenter; after dismantling and reassembling if the force, diameter measuring system or testing cycle are affected, after failure of indirect verification and when the last indirect verification was more than 13 months ago — force, diameter measuring system and testing cycle; it is recommended that the indenter be directly verified or replaced after 2 years of use. The verification report / calibration certificate gives, among other things: reference to ISO 6506-2, method of verification, identification of the machine, means of verification, ball diameter and force, temperature, result, date and institution, and the uncertainty of the results.
STATUS (PKN card, read 15.11.2026). PN-EN ISO 6506-2:2019-10 — English version, Polish title “Metale -- Pomiar twardości sposobem Brinella -- Część 2: Sprawdzanie i wzorcowanie twardościomierzy”, published 29-10-2019, 28 pages, KT 123 for Testing of Properties of Metals, implements EN ISO 6506-2:2018 and ISO 6506-2:2017 [IDT], replaces PN-EN ISO 6506-2:2014-12 (English and Polish versions); the card gives no withdrawal date. iTeh catalogue (15.11.2026): ISO 6506-2:2017 is at stage “International Standard to be revised” (90.92), and the European draft prEN ISO 6506-2 is at stage “decision to abandon — enquiry” (40.98).
IN ACCREDITATION SCOPES (scope database of the service, read 15.11.2026, after loading the scopes of this batch). PN-EN ISO 6506-2 appears at 9 Polish calibration laboratories (1 record each) — usually in the 2019-10 edition (at three written as “2019”), at four alongside ASTM E10-23, at two as the basis of an internal procedure — and at 5 Czech laboratories.
Method principle
The machine is verified in two ways. Directly — by measuring its components: the test forces with an instrument according to ISO 376 class 1 or better (each reading within ±1,0 % of the nominal force), the indenter balls (diameter, hardness ≥ 1 500 HV, density (14,8 ± 0,2) g/cm³), the indentation diameter measuring system (difference ≤ 0,5 %) and the testing cycle. Indirectly — by making five indentations on each of at least two reference blocks calibrated according to ISO 6506-3 and comparing the repeatability r_rel and the error E_rel with the permissible values of tables 2 and 3.
Applications
- Brinell hardness testing machines, stationary and portable — verification before first use, after repair and periodically (ISO 6506-2:2017, clauses 1 and 7)
- Each test force and each ball diameter used in testing (6.2)
- Machines that cannot meet the force–time profile — modified verification of force and cycle according to annex B (clause 1)
- In accreditation scopes: 9 Polish calibration laboratories and 5 Czech
Key parameters
| Parameter | Value |
|---|---|
| STATUS (PKN card, 15.11.2026) | PN-EN ISO 6506-2:2019-10 (English version, published 29-10-2019); implements EN ISO 6506-2:2018 and ISO 6506-2:2017; replaces PN-EN ISO 6506-2:2014-12 |
| Temperature (5.1.1, 6.1) | (23 ± 5) °C; outside this range — stated in the report |
| Test force (5.2) | 3 readings of each force, with a lever at ≥ 3 indenter positions; instrument ISO 376 cl. 1 or masses ±0,2 %; each reading ±1,0 % of the nominal force |
| Ball (5.3) | diameter tolerance: 10 mm ±0,005 mm, 5 mm ±0,004 mm, 2,5 mm ±0,003 mm, 1 mm ±0,003 mm; ≥ 1 500 HV; density (14,8 ± 0,2) g/cm³ |
| Diameter measuring system (5.4) | reading within ±0,5 %; ≥ 4 intervals of a stage micrometer, difference ≤ 0,5 %; projected area — error ≤ 1 %; ≥ 4 reference indentations, ≤ 0,5 % |
| Indirect verification (6.2–6.4) | each force and ball; ≥ 2 blocks according to ISO 6506-3 from different ranges; 5 indentations per block |
| Permissible values, ratio 30 (table 2) | < 250 HBW: r_rel 3,0 %, E_rel ±3,0 %; 250–450 HBW: 2,5 %, ±2,5 %; > 450 HBW: 2,0 %, ±2,0 % |
| Other ratios 15, 10, 5, ≤ 2,5 (table 3) | r_rel 3,0 %, E_rel ±3,0 % |
| Intervals (clause 7, table 4) | indirect ≥ once every 12 months and after direct; direct, among others, after failed indirect and when indirect was > 13 months ago |
| Coverage in accreditation scopes (read 15.11.2026) | 9 Polish calibration laboratories (9 records); 5 Czech |
Standard
- Standard number
- PN-EN ISO 6506-2:2019-10 (English version; implements EN ISO 6506-2:2018 and ISO 6506-2:2017 [IDT])
- Title (PL)
- Metale — Pomiar twardości sposobem Brinella — Część 2: Sprawdzanie i wzorcowanie twardościomierzy
- Title (EN)
- Metallic materials — Brinell hardness test — Part 2: Verification and calibration of testing machines
Step-by-step procedure
-
General conditions
Check of the machine set-up according to the manufacturer's instructions: guide, mounting of the ball holder, application of the force without shock or vibration, effect of the illumination on the diameter measurement (clause 4).
-
Test forces
Three readings of each force within the working range (with a lever at not less than three indenter positions); each reading within ±1,0 % of the nominal force (5.2).
-
Balls and diameter measuring system
At least two balls from a batch — diameter, hardness, density; calibration of the diameter measuring system on a stage micrometer and check on reference indentations (5.3–5.4).
-
Testing cycle
Conformity with the ISO 6506-1 cycle — at manufacture, after repair and in the cases of table 4 (5.5).
-
Indirect verification
For each force and ball at least two blocks; measurement of the reference indentation (when not immediately after direct verification); five indentations each; r_rel and E_rel against tables 2 and 3 (clause 6).
-
Report
Reference to ISO 6506-2, method, machine data, means of verification, ball and force, temperature, result, date, institution, uncertainty (clause 8; uncertainty — annex A).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Force-measuring instrument (5.2.3) | According to ISO 376, class 1 or better; or balancing against a force accurate to ±0,2 % (calibrated masses) | — |
| Stage micrometer and reference circular images (5.4) | Calibration of the indentation diameter measuring system — at least four intervals or four images for each objective | — |
| Reference blocks (6.1) | Calibrated according to ISO 6506-3, with certified hardness H_C and a reference indentation | — |
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN ISO 6506-2:2019-10 (English version; implements EN ISO 6506-2:2018 and ISO 6506-2:2017 [IDT]) — “Metallic materials — Brinell hardness test — Part 2: Verification and calibration of testing machines”.
How does this method work?
The machine is verified in two ways. Directly — by measuring its components: the test forces with an instrument according to ISO 376 class 1 or better (each reading within ±1,0 % of the nominal force), the indenter balls (diameter, hardness ≥ 1 500 HV, density (14,8 ± 0,2) g/cm³), the indentation diameter measuring system (difference ≤ 0,5 %) and the testing cycle.
What is the measuring range and accuracy?
STATUS (PKN card, 15.11.2026): PN-EN ISO 6506-2:2019-10 (English version, published 29-10-2019); implements EN ISO 6506-2:2018 and ISO 6506-2:2017; replaces PN-EN ISO 6506-2:2014-12; Temperature (5.1.1, 6.1): (23 ± 5) °C; outside this range — stated in the report; Test force (5.2): 3 readings of each force, with a lever at ≥ 3 indenter positions; instrument ISO 376 cl. 1 or masses ±0,2 %; each reading ±1,0 % of the nominal force; Ball (5.3): diameter tolerance: 10 mm ±0,005 mm, 5 mm ±0,004 mm, 2,5 mm ±0,003 mm, 1 mm ±0,003 mm; ≥ 1 500 HV; density (14,8 ± 0,2) g/cm³.
How long does the test take?
The procedure comprises 6 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.
What equipment is required?
Force-measuring instrument (5.2.3), Stage micrometer and reference circular images (5.4), Reference blocks (6.1).
Where is this test used?
Brinell hardness testing machines, stationary and portable — verification before first use, after repair and periodically (ISO 6506-2:2017, clauses 1 and 7); Each test force and each ball diameter used in testing (6.2); Machines that cannot meet the force–time profile — modified verification of force and cycle according to annex B (clause 1); In accreditation scopes: 9 Polish calibration laboratories and 5 Czech.
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 6506-2.