🔩 Metallic and inorganic coatings on metallic substrates after corrosion tests — rating of the protection rating Rp = 3(2 − log A) and the appearance rating RA on a 10–0 scale (A — % of the area with a defect), defect types A–J and severity vs/s/m/x, notation Rp/RA; PN-EN ISO 10289
In short
Rating of the condition of test specimens and articles with decorative and protective metallic and inorganic coatings on metallic substrates after exposure to the natural atmosphere or after accelerated corrosion tests. The test is performed according to PN-EN ISO 10289:2002 (Polish version; implements EN ISO 10289:2001 and ISO 10289:1999 [IDT]); STATUS (PKN card as of 13.11.2026): PN-EN ISO 10289:2002 current (Polish version, published 12-11-2002); implements EN ISO 10289:2001 and ISO 10289:1999; replaced PN-H-04633:1967. The procedure comprises 6 steps; it is used for: Decorative and protective metallic and inorganic coatings on metallic substrates — panels and articles after corrosion tests (ISO 10289:1999, clause 1), Exposure in natural atmospheres (mobile and static conditions) and accelerated tests (clause 1), Coatings anodic and cathodic to the substrate — the coating system has to be reported (introduction, clause 4).
At a glance
- Standard: PN-EN ISO 10289:2002 (Polish version; implements EN ISO 10289:2001 and ISO 10289:1999 [IDT])
- Category: Materials and NDT
- Procedure steps: 6
- STATUS (PKN card as of 13.11.2026): PN-EN ISO 10289:2002 current (Polish version, published 12-11-2002); implements EN ISO 10289:2001 and ISO 10289:1999; replaced PN-H-04633:1967
- Protection rating Rp (6.1): Rp = 3(2 − log₁₀ A); A — % of the area with basis metal corrosion; formula for A > 0,046 416 %; no corrosion = 10
- Scale — Table 1: 10 no defects; 9 up to 0,1 %; 8 up to 0,25 %; 7 up to 0,5 %; 6 up to 1,0 %; 5 up to 2,5 %; 4 up to 5,0 %; 3 up to 10 %; 2 up to 25 %; 1 up to 50 %; 0 above 50 %
Overview
WHAT THE STANDARD COVERS. According to clause 1 of ISO 10289:1999 the standard gives a method of evaluating the condition of decorative and protective metallic and inorganic coatings on panels or articles that have been exposed to corrosive environments for test or other purposes — in natural atmospheres, in mobile or static conditions, or in accelerated tests. According to the introduction, the ability of the coating to protect the basis metal from corrosion (protection rating Rp) and its ability to retain its integrity and appearance (appearance rating RA) are evaluated separately; the coating may be anodic or cathodic to the substrate, and the coating system has to be known and reported. Note 1 to clause 1: the protection rating can be assessed objectively, the assessment of appearance depends on many subjective factors.
ACCORDING TO THE TEXT OF ISO 10289:1999 — DEFINITIONS, PRINCIPLE, TYPES OF DEFECT, INSPECTION, RATINGS, TEST REPORT (foreword, introduction, clauses 1–7, beginning of Annex A). The standard was prepared by ISO/TC 107 (Metallic and other inorganic coatings), subcommittee SC 7 (Corrosion tests); first edition, it cancelled and replaced ISO 1462:1973, ISO 4540:1980 and ISO 8403:1991; Annexes A and B are informative. Definitions (clause 2): protection rating Rp — number from Table 1 assigned to the ability of the coating to protect the basis metal; protection defect — e.g. crater corrosion, pin-hole corrosion, corrosion stain from the substrate, blisters and other defects involving basis metal corrosion; appearance rating RA — number and symbols from Table 2; performance rating — notation Rp/RA; significant surface — part of the surface essential for appearance or serviceability. Principle (clause 3): the result of inspection is recorded as two separate ratings; when only Rp is required, RA may be omitted and a dash is written in its place (e.g. 10/–). Inspection (clause 5): the significant surface is indicated by drawings or marking; lighting as uniform as possible, without direct reflection from sun or clouds, various angles of inspection; after the test the specimens are inspected uncleaned, and if dirt or salt deposits mask the defects they may be sponged with a mild soap solution and rinsed with water without pressure (so as not to remove corrosion products and upgrade the rating); in intermediate, periodic inspections the specimens are not cleaned or disturbed; surfaces are dried before inspection. Only defects visible to normal or corrected vision count (optical aids only to characterize defects already detected). Edge defects within 5 mm of the edge of the specimen or of the tape/wax may be noted but normally do not influence the rating; contact and rack marks and mounting holes are disregarded; with a coating anodic to the substrate, white corrosion product from the edges does not constitute failure. Rubbing, polishing or chemical cleaning to study the surface — on the smallest practicable area, preferably not more than 100 mm² on a surface of 100 mm × 150 mm. Protection rating (6.1): Rp = 3(2 − log₁₀ A), where A is the percentage of the total area showing basis metal corrosion, rounded to the nearest whole number (Table 1); the formula is defined for A > 0,046 416 %, and a surface with no basis metal corrosion is assigned 10; fractional ratings may be used. Table 1 (Rp or RA): no defects — 10; 0 < A ≤ 0,1 — 9; 0,1 < A ≤ 0,25 — 8; 0,25 < A ≤ 0,5 — 7; 0,5 < A ≤ 1,0 — 6; 1,0 < A ≤ 2,5 — 5; 2,5 < A ≤ 5,0 — 4; 5,0 < A ≤ 10 — 3; 10 < A ≤ 25 — 2; 25 < A ≤ 50 — 1; A > 50 — 0. For very localized defects, dot charts or photographs (Annexes A and B) or flexible graticules with 1 mm, 2 mm or 5 mm squares may be used. For a large group of specimens — each rated individually by the formula, then the whole group is reviewed (arranged in order of merit) as a check that the inspector's judgement has not changed (lighting, fatigue). Appearance rating (6.2): type of defect according to Table 2, area affected by the defect on the 10–0 scale of Table 1 and subjective degree of severity: vs — very slight, s — slight, m — moderate, x — severe. Table 2: A — spotting and/or discoloration from coating deterioration (other than from basis metal corrosion products), B — tarnishing with little or no coating corrosion, C — corrosion products of an anodic coating, D — corrosion products of a cathodic coating, E — surface pitting (corrosion pits probably not reaching the basis metal), F — flaking, peeling, G — blistering, H — cracking, I — crazing, J — crow's-foot and star cracking. Examples of notation (6.3): 9/2 m A; 10/6 s C; 7/8 vs C, 6 m G. Test report (clause 7): test conditions, exposure period, description of the coating system and basis metal or of the product, any difficulty in assessing Rp, shape and dimensions of the specimens, surface preparation (cleaning, edge protection, deliberate damage), number of specimens, cleaning before rating, Rp and RA of each specimen.
STATUS (PKN card as of 13.11.2026). The card for PN-EN ISO 10289:2002 (Polish version) has no withdrawal label: title "Metody badań korozyjnych powłok metalowych i innych powłok nieorganicznych na podłożach metalowych -- Ocena próbek i wyrobów gotowych poddanych badaniom korozyjnym", published 12-11-2002, 27 pages, KT 106 for Corrosion and Corrosion Protection of Metallic Materials, "Implements: EN ISO 10289:2001 [IDT], ISO 10289:1999 [IDT]", "Replaces: PN-H-04633:1967", ICS 25.220.20, 25.220.40. ISO 10289:1999 in the iTeh catalogue — published, stage "International Standard under periodical review".
HOW MANY LABORATORIES AND IN WHAT FORM (accreditation scope database of the service, read 13.11.2026). The notation ISO 10289 appears in 5 records at 5 Polish laboratories: "PN-EN ISO 10289:2002" — AB 089 (together with PN-EN ISO 4628-1:2016-03), AB 1631 and AB 1700; "PN-EN ISO 10289" without a date — AB 910 (together with PN-EN ISO 4628-2 and PN-EN ISO 9227) and AB 904. Outside Poland — 7 Czech laboratories (ČSN EN ISO 10289, usually alongside standards of the ISO 4628 series).
WHAT THE LABORATORIES TEST (scope database, complete items — 5 Polish). Metallic coatings — "assessment of the protection and appearance ratings" (AB 1631); organic and inorganic (metallic, oxide) coatings on ferromagnetic and non-ferromagnetic substrates — protection rating, appearance rating, protection performance rating (AB 1700); metals, plastics, composites, organic and inorganic paint coatings — assessment of coating degradation (AB 089); protective coatings and metal products, including welded joints — corrosion resistance, accelerated method in salt spray (AB 910); finished products, components, metals and coatings — item described as geometric dimensions, direct measurement (AB 904). ISO 10289 concerns metallic and inorganic coatings — organic coatings (paints, varnishes) in the AB 089 and AB 1700 items are usually rated to ISO 4628, which these laboratories list alongside.
WHERE AN APPARENTLY CORRECT RESULT IS EASY TO GET. Cleaning: scrubbing or removing corrosion products before rating upgrades the rating (clause 5 allows only sponging without pressure); in periodic inspections specimens are not cleaned at all. Edges: defects within the 5 mm band from the edge and white corrosion product of an anodic coating from the edges counted as defects. Formula: Rp calculated for very small A (the result exceeds 10) — the formula is defined for A > 0,046 416 %. Anodic coatings: voluminous corrosion products of the coating (e.g. zinc on steel in a saline atmosphere) can mask substrate corrosion and make a reliable Rp impossible — this has to be recorded. Notation: no dash in place of an omitted RA, no type of defect and severity with RA.
WHAT WE DO NOT GIVE. Part read: the iTeh sample of ISO 10289:1999 in English (up to the beginning of 6.2) and French (clauses 1–7, beginning of Annex A — rules for using the dot charts). We do not give the content of the dot charts and photographs of Annexes A and B or the bibliography. We did not read the Polish text of PN-EN ISO 10289:2002.
Method principle
After the corrosion test or exposure, the significant surface of the specimen or article (uncleaned or only sponged) is inspected under uniform lighting and at various angles, disregarding the 5 mm band from the edges. The protection rating Rp is calculated from the percentage A of the area showing basis metal corrosion: Rp = 3(2 − log₁₀ A), rounded according to Table 1 (10 — no corrosion, 0 — A > 50 %). The appearance rating RA states the type of defect (A–J), its extent on the same 10–0 scale and the degree of severity (vs, s, m, x); the result is recorded as Rp/RA.
Applications
- Decorative and protective metallic and inorganic coatings on metallic substrates — panels and articles after corrosion tests (ISO 10289:1999, clause 1)
- Exposure in natural atmospheres (mobile and static conditions) and accelerated tests (clause 1)
- Coatings anodic and cathodic to the substrate — the coating system has to be reported (introduction, clause 4)
- In accreditation scopes: 5 Polish laboratories — metallic and inorganic coatings, products after salt spray; 7 Czech
Key parameters
| Parameter | Value |
|---|---|
| STATUS (PKN card as of 13.11.2026) | PN-EN ISO 10289:2002 current (Polish version, published 12-11-2002); implements EN ISO 10289:2001 and ISO 10289:1999; replaced PN-H-04633:1967 |
| Protection rating Rp (6.1) | Rp = 3(2 − log₁₀ A); A — % of the area with basis metal corrosion; formula for A > 0,046 416 %; no corrosion = 10 |
| Scale — Table 1 | 10 no defects; 9 up to 0,1 %; 8 up to 0,25 %; 7 up to 0,5 %; 6 up to 1,0 %; 5 up to 2,5 %; 4 up to 5,0 %; 3 up to 10 %; 2 up to 25 %; 1 up to 50 %; 0 above 50 % |
| Appearance rating RA (6.2) | type of defect A–J (Table 2) + extent on the 10–0 scale + severity vs, s, m, x |
| Result notation (2.5, 6.3) | Rp/RA, e.g. 9/2 m A; 7/8 vs C, 6 m G; Rp only — with a dash: 10/– |
| Edges (clause 5) | defects within 5 mm of the edge or of the tape/wax normally do not influence the rating |
| Area to be cleaned (clause 5) | preferably ≤ 100 mm² on a surface of 100 mm × 150 mm |
| Aids (6.1) | dot charts and photographs (Annexes A and B), flexible graticules with 1 mm, 2 mm or 5 mm squares |
| Coverage in accreditation scopes (database, read 13.11.2026) | 5 Polish laboratories, 5 records; 7 Czech |
Standard
- Standard number
- PN-EN ISO 10289:2002 (Polish version; implements EN ISO 10289:2001 and ISO 10289:1999 [IDT])
- Title (PL)
- Metody badań korozyjnych powłok metalowych i innych powłok nieorganicznych na podłożach metalowych — Ocena próbek i wyrobów gotowych poddanych badaniom korozyjnym
- Title (EN)
- Methods for corrosion testing of metallic and other inorganic coatings on metallic substrates — Rating of test specimens and manufactured articles subjected to corrosion tests
Step-by-step procedure
-
Before the test
Marking the significant surface; recording imperfections present before exposure and deliberate damage; protecting the edges with tape or wax if this is part of the test (clauses 1, 5).
-
Preparation for inspection
Specimens uncleaned; if necessary sponging with a mild soap solution without pressure and rinsing with water; drying the surface (clause 5).
-
Inspection
Uniform lighting, various angles; defects visible to normal or corrected vision; disregarding the 5 mm band from the edge, contact marks and mounting holes (clause 5).
-
Protection rating Rp
Share A of the area with substrate corrosion; Rp = 3(2 − log₁₀ A) rounded according to Table 1; for localized defects — standards or graticule (6.1).
-
Appearance rating RA and notation
Type of defect A–J, extent 10–0, severity vs/s/m/x; notation Rp/RA, with several defects — each separately; for a large group a review of the arrangement (6.2–6.3).
-
Test report
Exposure conditions and period, coating system and substrate, difficulties in assessing Rp, dimensions and preparation of the specimens, number of specimens, cleaning, Rp and RA of each specimen (clause 7).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Inspection lighting (clause 5) | As uniform as possible, without direct reflection from sun or clouds; inspection at various angles | — |
| Optical aids (clause 5, note 1) | To characterize defects already detected by eye — not to detect them | — |
| Standards for rating the area (6.1) | Dot charts or photographs of Annexes A and B; flexible graticules with 1 mm, 2 mm or 5 mm squares | — |
Reagents, media and consumables
| Reagent | CAS | Details |
|---|---|---|
| Mild soap solution and water (clause 5) | — | Only when dirt or salt deposits mask the defects: sponging without pressure and rinsing with water; cleaning agent compatible with the coating |
Health and safety (OHS)
- The standard contains no safety warning in the text read
- TECHNICAL NOTE: with anodic coatings (e.g. zinc on steel in a saline atmosphere) the corrosion products of the coating can mask substrate corrosion — a reliable Rp may be impossible (6.1, note 2)
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN ISO 10289:2002 (Polish version; implements EN ISO 10289:2001 and ISO 10289:1999 [IDT]) — “Methods for corrosion testing of metallic and other inorganic coatings on metallic substrates — Rating of test specimens and manufactured articles subjected to corrosion tests”.
How does this method work?
After the corrosion test or exposure, the significant surface of the specimen or article (uncleaned or only sponged) is inspected under uniform lighting and at various angles, disregarding the 5 mm band from the edges. The protection rating Rp is calculated from the percentage A of the area showing basis metal corrosion: Rp = 3(2 − log₁₀ A), rounded according to Table 1 (10 — no corrosion, 0 — A > 50 %).
What is the measuring range and accuracy?
STATUS (PKN card as of 13.11.2026): PN-EN ISO 10289:2002 current (Polish version, published 12-11-2002); implements EN ISO 10289:2001 and ISO 10289:1999; replaced PN-H-04633:1967; Protection rating Rp (6.1): Rp = 3(2 − log₁₀ A); A — % of the area with basis metal corrosion; formula for A > 0,046 416 %; no corrosion = 10; Scale — Table 1: 10 no defects; 9 up to 0,1 %; 8 up to 0,25 %; 7 up to 0,5 %; 6 up to 1,0 %; 5 up to 2,5 %; 4 up to 5,0 %; 3 up to 10 %; 2 up to 25 %; 1 up to 50 %; 0 above 50 %; Appearance rating RA (6.2): type of defect A–J (Table 2) + extent on the 10–0 scale + severity vs, s, m, x.
How long does the test take?
The procedure comprises 6 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.
What equipment is required?
Inspection lighting (clause 5), Optical aids (clause 5, note 1), Standards for rating the area (6.1).
Where is this test used?
Decorative and protective metallic and inorganic coatings on metallic substrates — panels and articles after corrosion tests (ISO 10289:1999, clause 1); Exposure in natural atmospheres (mobile and static conditions) and accelerated tests (clause 1); Coatings anodic and cathodic to the substrate — the coating system has to be reported (introduction, clause 4); In accreditation scopes: 5 Polish laboratories — metallic and inorganic coatings, products after salt spray; 7 Czech.
What safety precautions apply?
The standard contains no safety warning in the text read; TECHNICAL NOTE: with anodic coatings (e.g. zinc on steel in a saline atmosphere) the corrosion products of the coating can mask substrate corrosion — a reliable Rp may be impossible (6.1, note 2).
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 10289.