🔩 Resistance of unplasticized poly(vinyl chloride) PVC-U pipes to dichloromethane at a specified temperature (DCMT) — three pipe pieces 160 mm long, one end chamfered at 10°, 20° or 30° depending on wall thickness, immersed for (30 ± 1) min in dichloromethane under a water layer, result “no attack”; PN-EN ISO 9852

Materials and NDT PN-EN ISO 9852

In short

The resistance of PVC-U pipes to dichloromethane is checked by immersing chamfered pipe pieces 160 mm long for (30 ± 1) min in dichloromethane at the temperature T given in the referring standard (not lower than 12 °C), covered with a layer of water. The test is performed according to PN-EN ISO 9852:2017-11 (Polish version; implements EN ISO 9852:2017 and ISO 9852:2007 [IDT]); STATUS (as of 23.11.2026): PKN card: PN-EN ISO 9852:2017-11 — Polish version, published 06-12-2018, 14 pages, KT 140, implements EN ISO 9852:2017 [IDT] and ISO 9852:2007 [IDT], replaces PN-EN 580:2005 (Polish version); the card gives no withdrawal date. The procedure comprises 5 steps (about 25–30 min in total); it is used for: Unplasticized poly(vinyl chloride) PVC-U pipes irrespective of their intended use (clause 1), Rapid quality control during the manufacture of PVC-U pipes (clause 1), Test required by product standards, which give the temperature T, the minimum wall thickness and the number of test pieces (note 2 to clause 2).

At a glance

  • Standard: PN-EN ISO 9852:2017-11 (Polish version; implements EN ISO 9852:2017 and ISO 9852:2007 [IDT])
  • Category: Materials and NDT
  • Procedure steps: 5
  • Total time of stages: 25 min–30 min
  • STATUS (as of 23.11.2026): PKN card: PN-EN ISO 9852:2017-11 — Polish version, published 06-12-2018, 14 pages, KT 140, implements EN ISO 9852:2017 [IDT] and ISO 9852:2007 [IDT], replaces PN-EN 580:2005 (Polish version); the card gives no withdrawal date.
  • Immersion time (clause 2, 7.3): (30 ± 1) min in dichloromethane
  • Dichloromethane temperature (6.3): (T ± 0,5) °C, T from the referring standard, not less than 12 °C

Overview

WHAT THE STANDARD COVERS. According to clause 1 of ISO 9852:2007 the standard specifies a method for determining the resistance of unplasticized poly(vinyl chloride) (PVC-U) pipes to dichloromethane at a specified temperature (DCMT). It applies to all PVC-U pipes irrespective of their intended use and can be used as a rapid means of quality control during manufacture. The temperature of the dichloromethane up to which the pipe shall not be attacked is given in the referring standard.

ACCORDING TO THE TEXT OF ISO 9852:2007 (edition 2; the publisher's sample covers the foreword and clauses 1–8.1, without the rest of clause 8, clause 9 and the annexes). The standard was prepared by committee ISO/TC 138.

PRINCIPLE (clause 2). A piece of PVC-U pipe of specified length, chamfered at one end at an angle depending on the wall thickness, is immersed for (30 ± 1) min in dichloromethane at the temperature T given in the referring standard, to verify that the PVC-U is not attacked at that temperature. For safety reasons the surface of the dichloromethane is kept to a minimum and covered with a deep layer of water to reduce evaporation; after immersion the test piece drips in the water layer, then dries and is inspected. According to the note to clause 2, if the PVC-U is not sufficiently gelled, whitening of the surface occurs and, in the worst case, a precipitate. The referring standard sets: the temperature T, the minimum wall thickness for which the test can be used and — where appropriate — the number of test pieces.

REAGENT AND APPARATUS (clauses 3–4). Technical-grade dichloromethane; according to the note it contains small quantities (at most 1 % each) of chloromethane, trichloromethane and tetrachloromethane, and even 5 % of these impurities in total does not significantly affect the result. Chamfering machine; glass or stainless-steel container with a grating about 10 mm above the bottom (set at two levels: immersion in the dichloromethane or in the water layer only), a lid and temperature control with a stirrer, keeping the liquid at (T ± 0,5) °C; cooling equipment; hood with fume extraction over the container.

TEST PIECES (clause 5). Pieces 160 mm long are cut from the pipe under test, with ends perpendicular to the axis; unless the referring standard specifies otherwise — three. The wall thickness must be greater than the minimum given in the referring standard. One end of each piece is chamfered over the entire wall thickness by cutting (not grinding), without appreciable heating; the angle of chamfer according to Table 1: wall thickness e < 8 mm — 10°, 8 mm ≤ e < 16 mm — 20°, e ≥ 16 mm — 30°. Pieces larger than the diameter of the container are cut longitudinally into as few sections as possible (saw blade at most 2,5 mm wide) and cooled to ambient temperature.

IMMERSION CONDITIONS (clause 6). Dichloromethane of known refractive index is poured in so as to cover the whole chamfered zone and is covered with a layer of water preferably 250–300 mm deep, not less than 20 mm. The temperature of the dichloromethane is kept at (T ± 0,5) °C; it shall not be lower than 12 °C. Dichloromethane is topped up between tests, and its refractive index shall not vary during use by more than ± 0,002 from the initial value (according to the note it changes by about 0,000 5 in 3 months with 700–800 tests).

PROCEDURE (clause 7). The test pieces are not touched with the fingers (tongs, gloves). Each piece is placed so that the chamfered zone is completely immersed in the dichloromethane, for (30 ± 1) min; the grating is then raised for 10–15 min into the water layer to let the dichloromethane drip off. The pieces are dried in air until the water has evaporated, but for at least 15 min, in a well-ventilated area or under a hood with extraction, and inspected.

RESULT (8.1). If the test piece or all its sections show no sign of attack anywhere (other than swelling), the result is expressed as “no attack”.

WHERE A SEEMINGLY CORRECT RESULT IS EASY TO GET. The angle of chamfer is chosen for the wall thickness from Table 1 — a chamfer at another angle changes the surface tested; the chamfer is made by cutting without heating; the dichloromethane must keep its refractive index within ± 0,002 and the temperature within (T ± 0,5) °C — the standard does not allow a temperature below 12 °C.

WHAT WE DO NOT GIVE HERE. The rest of clause 8 (how the result is expressed when the test piece is attacked), clause 9 (test report) or Annexes A and B (figures of the chamfer and the container) — the sample ends at 8.1; the standard does not give the temperature T — it is set by the product standard.

STATUS (as of 23.11.2026). PKN card: PN-EN ISO 9852:2017-11 “Rury z nieplastyfikowanego poli(chlorku winylu) (PVC-U) -- Odporność na dichlorometan w określonej temperaturze (DCMT) -- Metoda badania” — Polish version, published 06-12-2018, 14 pages, KT 140 (plastics pipes, fittings and valves), implements EN ISO 9852:2017 [IDT] and ISO 9852:2007 [IDT], replaces PN-EN 580:2005 (Polish version); the card gives no withdrawal date. In accreditation scopes the method is sometimes cited together with PN-EN 580:2005 — according to the PKN card this is the standard replaced by PN-EN ISO 9852:2017-11.

Method principle

A chamfered piece of PVC-U pipe is immersed for 30 min in dichloromethane at the temperature from the product standard to check whether the PVC-U is attacked at that temperature; according to the note to clause 2, insufficiently gelled PVC-U shows whitening of the surface and, in the worst case, a precipitate.

Applications

Key parameters

ParameterValue
STATUS (as of 23.11.2026)PKN card: PN-EN ISO 9852:2017-11 — Polish version, published 06-12-2018, 14 pages, KT 140, implements EN ISO 9852:2017 [IDT] and ISO 9852:2007 [IDT], replaces PN-EN 580:2005 (Polish version); the card gives no withdrawal date.
Immersion time (clause 2, 7.3)(30 ± 1) min in dichloromethane
Dichloromethane temperature (6.3)(T ± 0,5) °C, T from the referring standard, not less than 12 °C
Test pieces (5.1)pipe pieces 160 mm long, ends perpendicular to the axis; three unless the referring standard specifies otherwise
Angle of chamfer — Table 1 (5.2)e < 8 mm: 10°; 8 mm ≤ e < 16 mm: 20°; e ≥ 16 mm: 30° (e — wall thickness); chamfer by cutting without heating
Water layer (6.2)preferably 250–300 mm, not less than 20 mm
Refractive index of dichloromethane (6.5)variation during use not more than ± 0,002 from the initial value
Dripping and drying (7.4, 7.5)10–15 min in the water layer; drying in air for at least 15 min in a ventilated area
Result (8.1)“no attack” when there is no sign of attack other than swelling

Standard

Standard number
PN-EN ISO 9852:2017-11 (Polish version; implements EN ISO 9852:2017 and ISO 9852:2007 [IDT])
Title (PL)
Rury z nieplastyfikowanego poli(chlorku winylu) (PVC-U) — Odporność na dichlorometan w określonej temperaturze (DCMT) — Metoda badania
Title (EN)
Unplasticized poly(vinyl chloride) (PVC-U) pipes — Dichloromethane resistance at specified temperature (DCMT) — Test method

Step-by-step procedure

  1. Test pieces

    Three pipe pieces 160 mm long, ends perpendicular to the axis; one end chamfered by cutting at the angle from Table 1; large pieces cut longitudinally; cooled to ambient temperature (5.1–5.4).

  2. Bath

    Dichloromethane covering the chamfered zone, with a water layer of 250–300 mm (at least 20 mm) above it; temperature (T ± 0,5) °C, not less than 12 °C (6.1–6.3).

    🌡 Temperature: (T ± 0,5) °C

  3. Immersion

    Test pieces handled with tongs, not touched with the fingers; chamfered zone completely in the dichloromethane (7.1–7.3).

    ⏱ Time: (30 ± 1) min

  4. Dripping

    Grating raised into the water layer so that the dichloromethane drips off (7.4).

    ⏱ Time: 10–15 min

  5. Drying and assessment

    Drying in air until the water has evaporated, at least 15 min, under extraction; inspection and record “no attack” when there is no sign of attack other than swelling (7.5–7.6, 8.1).

    ⏱ Time: at least 15 min

Required equipment and apparatus

EquipmentExampleIndicative price
Chamfering machine (4.1)Chamfer by cutting, without grinding and without appreciable heating (5.2)—
Container with grating and temperature control (4.2)Glass or stainless steel, grating about 10 mm above the bottom at two levels, lid, stirrer; keeps (T ± 0,5) °C—
Cooling equipment (4.3)Cools the dichloromethane to the temperature from the referring standard—
Hood with fume extraction (4.4)Over the container, for safety reasons—

Reagents, media and consumables

ReagentCASDetails
Technical-grade dichloromethane (3.1)—According to the note it contains at most 1 % each of chloromethane, trichloromethane and tetrachloromethane; refractive index known and checked (6.1, 6.5).

Health and safety (OHS)

Frequently asked questions

Which standard describes this test?

The test is performed according to PN-EN ISO 9852:2017-11 (Polish version; implements EN ISO 9852:2017 and ISO 9852:2007 [IDT]) — “Unplasticized poly(vinyl chloride) (PVC-U) pipes — Dichloromethane resistance at specified temperature (DCMT) — Test method”.

How does this method work?

A chamfered piece of PVC-U pipe is immersed for 30 min in dichloromethane at the temperature from the product standard to check whether the PVC-U is attacked at that temperature; according to the note to clause 2, insufficiently gelled PVC-U shows whitening of the surface and, in the worst case, a precipitate.

What is the measuring range and accuracy?

STATUS (as of 23.11.2026): PKN card: PN-EN ISO 9852:2017-11 — Polish version, published 06-12-2018, 14 pages, KT 140, implements EN ISO 9852:2017 [IDT] and ISO 9852:2007 [IDT], replaces PN-EN 580:2005 (Polish version); the card gives no withdrawal date.; Immersion time (clause 2, 7.3): (30 ± 1) min in dichloromethane; Dichloromethane temperature (6.3): (T ± 0,5) °C, T from the referring standard, not less than 12 °C; Test pieces (5.1): pipe pieces 160 mm long, ends perpendicular to the axis; three unless the referring standard specifies otherwise.

How long does the test take?

The times given for the individual stages add up to approximately 25 min–30 min. The procedure comprises 5 steps.

What equipment is required?

Chamfering machine (4.1), Container with grating and temperature control (4.2), Cooling equipment (4.3), Hood with fume extraction (4.4).

Where is this test used?

Unplasticized poly(vinyl chloride) PVC-U pipes irrespective of their intended use (clause 1); Rapid quality control during the manufacture of PVC-U pipes (clause 1); Test required by product standards, which give the temperature T, the minimum wall thickness and the number of test pieces (note 2 to clause 2).

What safety precautions apply?

According to the warning in clause 3 of the standard, dichloromethane has a low boiling point (40 °C) and hence a high vapour pressure at ambient temperature; it can be toxic by absorption through the skin and eyes, and its vapour is toxic — the standard gives a TLV/MAC value of 100 ml/m³ (ppm). Ventilation of the room in which the container stands and the test pieces dry is essential; the test pieces are not touched with the fingers (7.1).

Which laboratory can perform this test?

The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 9852.