⚡ Pressure test at high temperature for cable insulation and sheaths — blade with an edge of (0,70 ± 0,01) mm pressed with the force of Annex A, oven with natural air circulation ±2 K, free from vibration, 4 h (D ≤ 15 mm) or 6 h (D > 15 mm), rapid cooling under load, depth of indentation under a microscope as a percentage of thickness, median of three test pieces; PN-EN 60811-508
In short
The resistance of cable insulation and sheaths (mainly of thermoplastic compounds) to pressure at high temperature is tested by pressing a rectangular blade with an edge of (0,70 ± 0,01) mm against the test piece in an oven with natural air circulation, which maintains the temperature given in the cable standard to within ±2 K. The test is performed according to PN-EN 60811-508:2012 (English version; implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments PN-EN 60811-508:2012/A1:2018-02 (English version; implements EN 60811-508:2012/A1:2017 and IEC 60811-508:2012/AMD1:2017 [IDT]) and PN-EN 60811-508:2012/A2:2024-03 (English version); STATUS (as of 22.11.2026): PKN cards: PN-EN 60811-508:2012 (English version, published 01-10-2012, 21 pages, KT 53, implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments A1:2018-02 (changes 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 and Annex A) and A2:2024-03 (changes 4.2.1, 4.4.1, 4.4.2.1); the cards give no withdrawal date. The procedure comprises 5 steps (about 4 h in total); it is used for: Insulation and sheaths of cables made of thermoplastic compounds; crosslinked — when required by the cable standard (clause 1), Circular, flat and sector-shaped cores — mounting according to Figure 1 (4.3.2.1), Smooth sheaths, ridged sheaths, sheaths applied over armour or screen and flat cables (4.4).
At a glance
- Standard: PN-EN 60811-508:2012 (English version; implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments PN-EN 60811-508:2012/A1:2018-02 (English version; implements EN 60811-508:2012/A1:2017 and IEC 60811-508:2012/AMD1:2017 [IDT]) and PN-EN 60811-508:2012/A2:2024-03 (English version)
- Category: Electronics and EMC
- Procedure steps: 5
- Total time of stages: 4 h
- STATUS (as of 22.11.2026): PKN cards: PN-EN 60811-508:2012 (English version, published 01-10-2012, 21 pages, KT 53, implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments A1:2018-02 (changes 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 and Annex A) and A2:2024-03 (changes 4.2.1, 4.4.1, 4.4.2.1); the cards give no withdrawal date.
- Blade (4.2.2): rectangular, edge width (0,70 ± 0,01) mm (wording of edition 1.0 — clause changed by A1:2017, we have not read the text after the amendment)
- Oven (4.2.1): natural air circulation, free from vibration and without exposed heating elements; temperature of the cable standard ±2 K (wording of edition 1.0 — clause changed by A1:2017 and A2:2023, we have not read the text after the amendments)
Overview
WHAT THE STANDARD COVERS. According to clause 1 of IEC 60811-508:2012 the standard gives the procedure for a pressure test at high temperature, which typically applies to thermoplastic compounds used for insulating and sheathing materials. The method is principally intended for thermoplastic materials, but may be used for cross-linked materials when required by the cable standard; it is not recommended for thicknesses below 0,7 mm.
ACCORDING TO THE TEXT OF IEC 60811-508:2012 (edition 1.0, 2012-03; publisher's sample: clauses 1–5 without figures and annexes). The standard was prepared by IEC TC 20 and is used in conjunction with IEC 60811-100:2012. It applies with amendments AMD1:2017 and AMD2:2023 (consolidated version IEC 60811-508:2012+AMD1:2017+AMD2:2023 CSV, edition 1.2); according to its foreword the significant technical changes are a re-statement of the oven characteristics (especially anti-vibration and temperature control), enhanced detail on the preparation and testing of flat cables and on thickness and dimensional measurements. According to the PKN card, amendment A1:2018-02 changes clauses 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 (Figure 4) and Annex A — we have not read their wording after the amendments, so the description below reflects the text of edition 1.0.
APPARATUS (4.2). The test is carried out in an oven with natural air circulation, without any equipment likely to cause vibration and without exposed heating elements, located in a position free from vibration; the oven shall maintain the temperature of the cable standard to within ±2 K — the standard stresses that for thermoplastics with a sharp melting point (e.g. some ethylene polymers) a small temperature rise results in a large increase in indentation. The indentation device (Figure 1) has a rectangular blade with an edge (0,70 ± 0,01) mm wide pressed against the test piece by an applied force.
INSULATION (4.3). All tests are carried out not less than 16 h after extrusion of the compound. From each core three adjacent pieces 50 mm to 100 mm long are taken from a sample of 250 mm to 500 mm; coverings and the semi-conducting layer are removed mechanically; the test piece has a length of (45 ± 5) mm. The cores of unsheathed flat cables are not separated, unless the conductor cross-section is at least 10 mm². The minimum insulation thickness to be tested is 0,7 mm (testing from 0,4 mm is possible but not recommended and is recorded in the test report). The force calculated according to Annex A is applied perpendicular to the axis of the core, and the blade is also perpendicular. The loaded blade is placed on the test piece at ambient temperature and the whole assembly is put into the oven at the test temperature; the temperature shall not at any time exceed the upper limit (brief drops below the lower limit just after the start are ignored). Time — from the cable standard, and if not specified: 4 h for D ≤ 15 mm and 6 h for D > 15 mm (D according to Annex A). After this time the test piece is rapidly cooled under load, e.g. by spraying cold water on the spot where the blade presses, and after cooling further in cold water.
MEASUREMENT AND RESULT (4.3.2.5–4.3.2.6). From the test piece (after withdrawal of the conductor) a narrow strip is cut along the axis, perpendicular to the indentation, and under a measuring microscope or projector the cross-wire is set to the bottom of the indentation and to the outer surface; test pieces up to about 6 mm in diameter are cut transversely at and adjacent to the indentation, and the depth is the difference between the two measurements. Measurements in millimetres to two decimal places. If the apparent thickness after the test (δ1) differs from the original one (δ), the measured indentation M is corrected: (M − (δ1 − δ)) / δ × 100. The indentations of the three test pieces are expressed as a percentage of the insulation thickness and the median is recorded; for flat cables the median is the mean of all cores of the same size. In the absence of a requirement in the cable standard, Annex B gives a recommendation.
SHEATHS (4.4). From a sample of 250 mm to 500 mm (after removal of the internal parts) three pieces of 50 mm to 100 mm are taken and a strip about one third of the perimeter wide, but not more than 20 mm, is cut parallel to the axis; with ridges from five or fewer cores the strip contains a groove in the middle, with more than five cores the ridges are ground off. The strip is supported by a metal mandrel with a radius of about half the inner diameter of the test piece; a sheath applied directly over an armour, screen or concentric conductor is not removed and the whole cable piece is tested. Flat cables with flat smaller sides — a strip 10 mm to 20 mm wide from the wide side, bent around a mandrel over at least 120° of its circumference. The rest as for insulation.
WHAT WE DO NOT GIVE HERE. We do not reproduce the formula for the compressing force from Annex A, the recommended indentation limit from Annex B, the figures or the wording of the clauses changed by AMD1:2017 and AMD2:2023, because they are not in the texts we read; the standard gives no test temperature — it is in the cable product standard.
STATUS (as of 22.11.2026). PKN cards: PN-EN 60811-508:2012 “Kable i przewody elektryczne oraz światłowodowe -- Metody badań materiałów niemetalowych -- Część 508: Badania mechaniczne -- Sprawdzenie odporności izolacji i powłok na nacisk w podwyższonej temperaturze” — English version, published 01-10-2012, 21 pages, KT 53 (cables and wires), implements EN 60811-508:2012 [IDT] and IEC 60811-508:2012 [IDT], replaces PN-EN 60811-3-1:1999 and PN-EN 60811-3-1:1999/A2:2002 (Polish versions); PN-EN 60811-508:2012/A1:2018-02 — English version, published 01-02-2018, 12 pages, changes 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 (Figure 4) and Annex A; PN-EN 60811-508:2012/A2:2024-03 — English version, published 08-03-2024, 10 pages, changes 4.2.1, 4.4.1 and 4.4.2.1. Neither card gives a withdrawal date.
Method principle
A rectangular blade loaded with the force of Annex A is placed at ambient temperature on a supported and fixed test piece of cable insulation or sheath, the assembly is kept in an oven at the temperature of the cable standard, rapidly cooled under load, and the depth of indentation is measured under a microscope as a percentage of the thickness.
Applications
- Insulation and sheaths of cables made of thermoplastic compounds; crosslinked — when required by the cable standard (clause 1)
- Circular, flat and sector-shaped cores — mounting according to Figure 1 (4.3.2.1)
- Smooth sheaths, ridged sheaths, sheaths applied over armour or screen and flat cables (4.4)
Key parameters
| Parameter | Value |
|---|---|
| STATUS (as of 22.11.2026) | PKN cards: PN-EN 60811-508:2012 (English version, published 01-10-2012, 21 pages, KT 53, implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments A1:2018-02 (changes 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 and Annex A) and A2:2024-03 (changes 4.2.1, 4.4.1, 4.4.2.1); the cards give no withdrawal date. |
| Blade (4.2.2) | rectangular, edge width (0,70 ± 0,01) mm (wording of edition 1.0 — clause changed by A1:2017, we have not read the text after the amendment) |
| Oven (4.2.1) | natural air circulation, free from vibration and without exposed heating elements; temperature of the cable standard ±2 K (wording of edition 1.0 — clause changed by A1:2017 and A2:2023, we have not read the text after the amendments) |
| Time in the oven (4.3.2.3) | from the cable standard; if not specified — 4 h for D ≤ 15 mm, 6 h for D > 15 mm |
| Test pieces (4.3.1, 4.4.1) | three adjacent pieces of 50 mm to 100 mm from a sample of 250 mm to 500 mm; insulation test piece (45 ± 5) mm; sheath strip up to 20 mm |
| Minimum thickness (4.3.1) | 0,7 mm (from 0,4 mm not recommended, with a note in the test report) |
| Measurement of indentation (4.3.2.5) | measuring microscope or projector, mm to two decimal places; correction (M − (δ1 − δ)) / δ × 100 (wording of edition 1.0 — clause changed by A1:2017, we have not read the text after the amendment) |
| Result (4.3.2.6) | median of three indentations in % of thickness; flat cables — mean of the cores of the same size |
Standard
- Standard number
- PN-EN 60811-508:2012 (English version; implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments PN-EN 60811-508:2012/A1:2018-02 (English version; implements EN 60811-508:2012/A1:2017 and IEC 60811-508:2012/AMD1:2017 [IDT]) and PN-EN 60811-508:2012/A2:2024-03 (English version)
- Title (PL)
- Kable i przewody elektryczne oraz światłowodowe — Metody badań materiałów niemetalowych — Część 508: Badania mechaniczne — Sprawdzenie odporności izolacji i powłok na nacisk w podwyższonej temperaturze
- Title (EN)
- Electric and optical fibre cables — Test methods for non-metallic materials — Part 508: Mechanical tests — Pressure test at high temperature for insulation and sheaths
Step-by-step procedure
-
Test pieces
Not less than 16 h after extrusion; three adjacent pieces of 50 mm to 100 mm, coverings and semi-conducting layer removed mechanically, test piece (45 ± 5) mm; sheaths — strip up to 20 mm (4.1, 4.3.1, 4.4.1).
-
Fixing and loading
Test piece fixed on the support so that it neither moves nor curves; force of Annex A perpendicular to the axis of the core, blade perpendicular (4.3.2.1, 4.3.2.2).
-
Oven
Loaded blade placed at ambient temperature, assembly into the oven at the test temperature; 4 h (D ≤ 15 mm) or 6 h (D > 15 mm) if the cable standard gives no time (4.3.2.3).
-
Cooling
Rapid cooling under load by spraying cold water on the spot of pressure, then in cold water (4.3.2.4).
-
Measurement and result
Strip cut along the axis perpendicular to the indentation, measurement under a microscope to 0,01 mm; indentation in % of thickness, median of three test pieces (4.3.2.5, 4.3.2.6).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Oven (4.2.1) | Natural air circulation, without equipment causing vibration and without exposed heating elements; ±2 K; located in a position free from vibration | — |
| Indentation device (4.2.2, Figure 1) | Rectangular blade with an edge of (0,70 ± 0,01) mm pressed by an applied force | — |
| Measuring microscope or projector (4.3.2.5) | With cross-wire; reading in millimetres to two decimal places | — |
| Metal mandrel (4.4.2.1) | Support for the sheath strip, radius about half the inner diameter of the test piece; may be halved along its axis | — |
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN 60811-508:2012 (English version; implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments PN-EN 60811-508:2012/A1:2018-02 (English version; implements EN 60811-508:2012/A1:2017 and IEC 60811-508:2012/AMD1:2017 [IDT]) and PN-EN 60811-508:2012/A2:2024-03 (English version) — “Electric and optical fibre cables — Test methods for non-metallic materials — Part 508: Mechanical tests — Pressure test at high temperature for insulation and sheaths”.
How does this method work?
A rectangular blade loaded with the force of Annex A is placed at ambient temperature on a supported and fixed test piece of cable insulation or sheath, the assembly is kept in an oven at the temperature of the cable standard, rapidly cooled under load, and the depth of indentation is measured under a microscope as a percentage of the thickness.
What is the measuring range and accuracy?
STATUS (as of 22.11.2026): PKN cards: PN-EN 60811-508:2012 (English version, published 01-10-2012, 21 pages, KT 53, implements EN 60811-508:2012 and IEC 60811-508:2012 [IDT]) with amendments A1:2018-02 (changes 4.2.1, 4.2.2, 4.3.2.5, 4.4.1, clause 5 and Annex A) and A2:2024-03 (changes 4.2.1, 4.4.1, 4.4.2.1); the cards give no withdrawal date.; Blade (4.2.2): rectangular, edge width (0,70 ± 0,01) mm (wording of edition 1.0 — clause changed by A1:2017, we have not read the text after the amendment); Oven (4.2.1): natural air circulation, free from vibration and without exposed heating elements; temperature of the cable standard ±2 K (wording of edition 1.0 — clause changed by A1:2017 and A2:2023, we have not read the text after the amendments); Time in the oven (4.3.2.3): from the cable standard; if not specified — 4 h for D ≤ 15 mm, 6 h for D > 15 mm.
How long does the test take?
The times given for the individual stages add up to approximately 4 h. The procedure comprises 5 steps.
What equipment is required?
Oven (4.2.1), Indentation device (4.2.2, Figure 1), Measuring microscope or projector (4.3.2.5), Metal mandrel (4.4.2.1).
Where is this test used?
Insulation and sheaths of cables made of thermoplastic compounds; crosslinked — when required by the cable standard (clause 1); Circular, flat and sector-shaped cores — mounting according to Figure 1 (4.3.2.1); Smooth sheaths, ridged sheaths, sheaths applied over armour or screen and flat cables (4.4).
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN 60811-508.