🔩 Injection-moulded thermoplastics fittings — visual assessment of the effects of heating: method A in an air-circulating oven (reference method) or method B in a liquid bath, 150 °C (PE 110 °C) ± 2 °C, 15–240 min depending on the mean wall thickness, cutting while hot, cracks, blisters, delaminations and fusion-line openings as % of the wall thickness; PN-EN ISO 580

Materials and NDT PN-EN ISO 580

In short

Assessment of the effects of heating on injection-moulded thermoplastics pipe fittings — method A in an air-circulating oven (the reference method in case of disagreement) or method B in a liquid bath. The test is performed according to PN-EN ISO 580:2006 (Polish version; implements EN ISO 580:2005 and ISO 580:2005 [IDT]); STATUS (PKN card as of 12.11.2026): PN-EN ISO 580:2006 current (Polish version, published 23-08-2006); implements EN ISO 580:2005 and ISO 580:2005; replaced the English edition PN-EN ISO 580:2005. The procedure comprises 5 steps (about 15 min–4 h in total); it is used for: Injection-moulded thermoplastics pipe fittings — cement-welded, flanged, with seals, assembled; pressure and non-pressure (ISO 580:2005, clause 1), Distinguishing properly from improperly moulded fittings: cold slugs, cavities, porosity, moulded-in stress, contamination, fusion line (introduction), Materials in Table 1: ABS, PE, PP, PVC-U, PVC-C, SAN+PVC.

At a glance

  • Standard: PN-EN ISO 580:2006 (Polish version; implements EN ISO 580:2005 and ISO 580:2005 [IDT])
  • Category: Materials and NDT
  • Procedure steps: 5
  • Total time of stages: 15 min–4 h
  • STATUS (PKN card as of 12.11.2026): PN-EN ISO 580:2006 current (Polish version, published 23-08-2006); implements EN ISO 580:2005 and ISO 580:2005; replaced the English edition PN-EN ISO 580:2005
  • Temperature — Table 1: T ± 2 °C: ABS 150 °C; PE 110 °C; PP, PVC-U, PVC-C, SAN+PVC 150 °C (when the referring standard does not specify otherwise)
  • Time — Table 1: em ≤ 3 mm — 15 min; 3–10 mm — 30 min; 10–20 mm — 60 min; 20–30 mm — 140 min; 30–40 mm — 220 min; > 40 mm — 240 min

Overview

WHAT THE STANDARD COVERS. According to clause 1 of ISO 580:2005 the standard specifies two methods for assessing the effects of heating on injection-moulded thermoplastics pipe fittings: method A in an air oven and method B in a liquid bath; in case of disagreement method A is the reference method. It applies to cement-welded and flanged fittings, fittings with elastomeric seals and fittings assembled from several mouldings (e.g. union connectors), pressure and non-pressure. Introduction: the test distinguishes properly from improperly moulded fittings — it reveals cold slugs and unfused areas, cavities and porosity, moulded-in stress, contamination and the integrity of the fusion line.

ACCORDING TO THE TEXT OF ISO 580:2005 — PRINCIPLE, PARAMETERS, METHODS A AND B, TEST REPORT (foreword, introduction, clauses 1–6). Third edition of 2005-02-15. Parameters (clause 3, Table 1 — when the referring standard does not specify otherwise): temperature T ± 2 °C — ABS 150 °C, PE 110 °C, PP, PVC-U, PVC-C and SAN+PVC 150 °C; time t depending on the mean wall thickness em: em ≤ 3 mm — 15 min, 3 < em ≤ 10 — 30 min, 10 < em ≤ 20 — 60 min, 20 < em ≤ 30 — 140 min, 30 < em ≤ 40 — 220 min, em > 40 mm — 240 min. Method A (clause 4): air-circulating oven maintaining the temperature of the working zone and regaining it within 15 min after insertion of the test pieces; thermometer graduated in 0.5 °C or a type T thermocouple (resolution 0.1 °C, accuracy at least ± 0.8 °C). Test pieces — complete mouldings without runners, without sealing rings, assembled fittings separated; number according to the product standard, in its absence at least three. The test pieces stand on a socket, not touching each other or the sides; time t is counted from the return of the temperature and chosen for the thickest part. Cuts while hot with a sharp knife or razor blade: dn ≤ 160 mm — at least two, dn > 160 mm — at least four, equally spaced around each socket or spigot. Examination (4.3.6): defects in the gating area as % of the wall thickness — for sprue gating within radius R according to the referring standard, in its absence R = 0.3 dn (maximum 50 mm); for ring or diaphragm gating within a length L = 0.3 dn (for cracks through the whole wall also their length); for fusion lines — the widest and deepest opening; outside the gating area — cracks, blisters and delaminations. Method B (clause 5): thermostatically controlled bath (T ± 2) °C with a liquid stable at that temperature, not affecting the test piece and safe — glycerine, glycol, mineral oil free from aromatic hydrocarbons or a calcium chloride solution (for ABS not glycol but mineral oil); holder not causing distortion; the composition of the liquid is given in the test report.

STATUS (PKN cards as of 12.11.2026). The card for PN-EN ISO 580:2006 (Polish version) has no withdrawal label: published 23-08-2006, 11 pages, KT 140 for Plastics Pipes, Fittings and Valves, "Implements: EN ISO 580:2005 [IDT], ISO 580:2005 [IDT]", "Replaces: PN-EN ISO 580:2005 - English version", ICS 23.040.45. The card for PN-EN ISO 580:2005 (English version): "Withdrawn and replaced by" PN-EN ISO 580:2006, withdrawal date 23-08-2006; it replaced PN-EN 763:1998. ISO 580:2005 in the iTeh catalogue — published.

HOW MANY LABORATORIES AND IN WHAT FORM (accreditation scope database of the service, read 12.11.2026). The notation ISO 580 appears in 5 records at 5 Polish laboratories: "PN-EN ISO 580:2006" — AB 005 (together with PN-ISO 12091:2009), AB 163, AB 237 (together with PN-ISO 12091:2009) and AB 1256; "PN-EN ISO 580" undated — AB 023. The item "PN-EN 580:2005" at AB 1256 (PVC-U pipes, resistance to dichloromethane) is not counted — it is a different standard. Outside Poland — 2 Czech laboratories (1004 and 1234, ČSN EN ISO 580).

WHAT THE LABORATORIES TEST (scope database, complete items — 5 Polish). Injection-moulded thermoplastics fittings up to a test piece size of 500 × 500 × 500 mm — "visual method, method A – heating in air, maximum temperature 200 °C" (AB 1256); injection-moulded thermoplastics fittings up to (400 × 400 × 490) mm and thermoplastics pipes up to 800 mm (AB 237); plastics pipes and fittings (AB 163); injection-moulded thermoplastics pipes and fittings (AB 023); pipes, pipe fittings with a diameter below 400 mm and other plastics products (AB 005). Pipes and "other products" go beyond the scope of ISO 580, which concerns injection-moulded fittings.

WHERE AN APPARENTLY CORRECT RESULT IS EASY TO GET. Parameters: time chosen for the mean wall thickness of the whole fitting instead of the thickest part; time counted from insertion instead of from the return of the temperature; an oven that does not regain the temperature within 15 min. Test pieces: sealing ring left in place, assembled fitting not taken apart, runners left on. Examination: cuts made cold or too few cuts (two for dn ≤ 160 mm, four above), gating area measured outside the radius R = 0.3 dn (maximum 50 mm) or the length L = 0.3 dn. Method B: a liquid that affects the plastic (glycol for ABS), no composition of the liquid in the report; in case of disagreement method A decides.

WHAT WE DO NOT GIVE. Part read: the iTeh sample of ISO 580:2005 in English and French (foreword, introduction, clauses 1–6); Table 1 was read from the page image. We do not give the content of the informative Annex A (guidance for the examination of a test piece), to which 4.3.6 refers — it is not in the sample — nor Figure 1 apart from the names of the gating types. We did not read the Polish text of PN-EN ISO 580:2006.

Method principle

Complete mouldings (without runners and sealing rings, assembled fittings separated) are heated at T ± 2 °C — 150 °C for ABS, PP, PVC-U, PVC-C and SAN+PVC, 110 °C for PE — in an air-circulating oven (method A, reference) or in a liquid bath (method B) for a time t from 15 min (em ≤ 3 mm) to 240 min (em > 40 mm), counted from the return of the temperature and chosen for the thickest part. Sockets and spigots are cut while hot (2 cuts for dn ≤ 160 mm, 4 above), and after cooling the surfaces and gating areas are examined; cracks, blisters, delaminations and fusion-line openings are expressed as a percentage of the wall thickness.

Applications

Key parameters

ParameterValue
STATUS (PKN card as of 12.11.2026)PN-EN ISO 580:2006 current (Polish version, published 23-08-2006); implements EN ISO 580:2005 and ISO 580:2005; replaced the English edition PN-EN ISO 580:2005
Temperature — Table 1T ± 2 °C: ABS 150 °C; PE 110 °C; PP, PVC-U, PVC-C, SAN+PVC 150 °C (when the referring standard does not specify otherwise)
Time — Table 1em ≤ 3 mm — 15 min; 3–10 mm — 30 min; 10–20 mm — 60 min; 20–30 mm — 140 min; 30–40 mm — 220 min; > 40 mm — 240 min
Oven — method A (4.1)air circulation, temperature regained in ≤ 15 min; thermometer graduated in 0.5 °C or type T thermocouple (0.1 °C, ± 0.8 °C)
Bath — method B (5.1)T ± 2 °C; glycerine, glycol, mineral oil free from aromatics or CaCl2 solution; for ABS not glycol
Test pieces (4.2)complete mouldings without runners and seals; according to the product standard, in its absence ≥ 3
Cuts while hot (4.3.5)dn ≤ 160 mm — ≥ 2; dn > 160 mm — ≥ 4, equally spaced around each socket or spigot
Gating area (4.3.6)sprue gating R = 0.3 dn (≤ 50 mm); ring/diaphragm gating L = 0.3 dn — when the referring standard does not specify otherwise
Coverage in accreditation scopes (database, read 12.11.2026)5 Polish laboratories, 5 records; 2 Czech

Standard

Standard number
PN-EN ISO 580:2006 (Polish version; implements EN ISO 580:2005 and ISO 580:2005 [IDT])
Title (PL)
Systemy przewodów rurowych i rur osłonowych z tworzyw sztucznych — Kształtki wtryskowe z tworzyw termoplastycznych — Metody wizualnej oceny zmian w wyniku ogrzewania
Title (EN)
Plastics piping and ducting systems — Injection-moulded thermoplastics fittings — Methods for visually assessing the effects of heating

Step-by-step procedure

  1. Parameters and test pieces

    T, t, number of test pieces, method and criteria according to the referring standard or Table 1; complete mouldings without runners and sealing rings, assembled fittings separated; ≥ 3 test pieces (clause 3, 4.2).

  2. Heating — method A or B

    Oven (A) or bath (B) at T ± 2 °C; test pieces on a socket, not touching; time t according to em of the thickest part, counted from the return of the temperature (4.3.1–4.3.3, 5.3.1–5.3.3).

    ⏱ Time: 15–240 min • 🌡 Temperature: 150 °C (PE 110 °C) ± 2 °C

  3. Removal and cutting while hot

    Without deformation; cuts with a sharp knife — ≥ 2 (dn ≤ 160 mm) or ≥ 4 (dn > 160 mm) around sockets and spigots; cooling in air (4.3.4–4.3.5).

  4. Examination

    Cracks, delaminations, fusion-line openings, blisters in the wall; in the gating area — within radius R = 0.3 dn (≤ 50 mm) or length L = 0.3 dn; defects as % of the wall thickness (4.3.6).

  5. Test report

    Standard and referring standard, fittings, method (B — composition of the liquid), temperature, duration, number of mouldings, changes in appearance, maximum dimensions of defects as % of the wall thickness, date (clause 6).

Required equipment and apparatus

EquipmentExampleIndicative price
Air-circulating oven — method A (4.1.1)Thermostatically controlled; maintains the test temperature in the working zone and regains it within 15 min after insertion of the test pieces—
Liquid bath and holder — method B (5.1.1–5.1.2)Thermostatically controlled (T ± 2) °C, agitated; holder supporting the fittings without additional distortion—
Thermometer (4.1.2, 5.1.3)Graduated in 0.5 °C or type T thermocouple with a resolution of 0.1 °C and an accuracy of at least ± 0.8 °C—
Knife or razor blade (4.3.5)Sharp — for cutting the test pieces while hot—

Reagents, media and consumables

ReagentCASDetails
Bath liquid — method B—Stable at the test temperature, not affecting the test piece, safe: glycerine, glycol, mineral oil free from aromatic hydrocarbons or calcium chloride solution; all suitable for PVC-U, for ABS mineral oil instead of glycol (note 1 to 5.1.1)

Health and safety (OHS)

Frequently asked questions

Which standard describes this test?

The test is performed according to PN-EN ISO 580:2006 (Polish version; implements EN ISO 580:2005 and ISO 580:2005 [IDT]) — “Plastics piping and ducting systems — Injection-moulded thermoplastics fittings — Methods for visually assessing the effects of heating”.

How does this method work?

Complete mouldings (without runners and sealing rings, assembled fittings separated) are heated at T ± 2 °C — 150 °C for ABS, PP, PVC-U, PVC-C and SAN+PVC, 110 °C for PE — in an air-circulating oven (method A, reference) or in a liquid bath (method B) for a time t from 15 min (em ≤ 3 mm) to 240 min (em > 40 mm), counted from the return of the temperature and chosen for the thickest part. Sockets and spigots are cut while hot (2 cuts for dn ≤ 160 mm, 4 above), and after cooling the surfaces and gating areas are examined; cracks, blisters, delaminations and fusion-line openings are expressed as a percentage of the wall thickness.

What is the measuring range and accuracy?

STATUS (PKN card as of 12.11.2026): PN-EN ISO 580:2006 current (Polish version, published 23-08-2006); implements EN ISO 580:2005 and ISO 580:2005; replaced the English edition PN-EN ISO 580:2005; Temperature — Table 1: T ± 2 °C: ABS 150 °C; PE 110 °C; PP, PVC-U, PVC-C, SAN+PVC 150 °C (when the referring standard does not specify otherwise); Time — Table 1: em ≤ 3 mm — 15 min; 3–10 mm — 30 min; 10–20 mm — 60 min; 20–30 mm — 140 min; 30–40 mm — 220 min; > 40 mm — 240 min; Oven — method A (4.1): air circulation, temperature regained in ≤ 15 min; thermometer graduated in 0.5 °C or type T thermocouple (0.1 °C, ± 0.8 °C).

How long does the test take?

The times given for the individual stages add up to approximately 15 min–4 h. The procedure comprises 5 steps.

What equipment is required?

Air-circulating oven — method A (4.1.1), Liquid bath and holder — method B (5.1.1–5.1.2), Thermometer (4.1.2, 5.1.3), Knife or razor blade (4.3.5).

Where is this test used?

Injection-moulded thermoplastics pipe fittings — cement-welded, flanged, with seals, assembled; pressure and non-pressure (ISO 580:2005, clause 1); Distinguishing properly from improperly moulded fittings: cold slugs, cavities, porosity, moulded-in stress, contamination, fusion line (introduction); Materials in Table 1: ABS, PE, PP, PVC-U, PVC-C, SAN+PVC; In accreditation scopes: 5 Polish laboratories — injection-moulded fittings, and also pipes and other plastics products.

What safety precautions apply?

The bath liquid (method B) must not cause any safety or health risks — the standard draws attention to relevant legislation (5.1.1, note 2); Test pieces are cut while hot with a sharp knife or razor blade (4.3.5) — work with hot mouldings (up to 150 °C) and a sharp tool; TECHNICAL NOTE: in case of disagreement between methods A and B, method A decides (clause 1).

Which laboratory can perform this test?

The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 580.

🔍 Find a laboratory performing this test