🏗️ Natural stone — water absorption at atmospheric pressure: at least 6 specimens (cube, cylinder or prism 70 mm or 50 mm, ≥ 60 ml), drying to constant mass at (70 ± 5) °C, immersion in stages (½ of the height, after 60 min ¾, after 120 min completely under 25 mm of water), weighing every 24 h to constant mass (difference ≤ 0,1 %), Ab = (ms − md)/md · 100 % to the nearest 0,1 %; PN-EN 13755
In short
Determination of the water absorption of natural stone by immersion in water at atmospheric pressure. The test is performed according to PN-EN 13755:2008 (English version; implements EN 13755:2008 [IDT]); STATUS (PKN card as of 13.11.2026): PN-EN 13755:2008 current (English version, published 25-06-2008); implements EN 13755:2008; replaced PN-EN 13755:2002 and AC:2004. The procedure comprises 6 steps (about 2 days 2 h in total); it is used for: Natural stone — water absorption by immersion at atmospheric pressure (EN 13755:2008, clause 1), A standard from the series of CEN/TC 246 test methods for natural stone (foreword), Specimens for compressive or flexural strength tests — if they meet the surface-to-volume ratio (6.2, note).
At a glance
- Standard: PN-EN 13755:2008 (English version; implements EN 13755:2008 [IDT])
- Category: Construction
- Procedure steps: 6
- Total time of stages: 2 days 2 h
- STATUS (PKN card as of 13.11.2026): PN-EN 13755:2008 current (English version, published 25-06-2008); implements EN 13755:2008; replaced PN-EN 13755:2002 and AC:2004
- Specimens (6.1–6.2): ≥ 6 from a homogeneous batch; cylinder, cube or prism (70 ± 5) mm or (50 ± 5) mm; ≥ 60 ml; surface/volume 0,08–0,20 mm⁻¹
- Drying (6.3): (70 ± 5) °C to constant mass (difference ≤ 0,1 % at an interval of (24 ± 2) h); cooling in a desiccator to (20 ± 5) °C
Overview
WHAT THE STANDARD COVERS. According to clause 1 of EN 13755:2008 the standard specifies a method for determining the water absorption of natural stone (terminology — EN 12670, denomination — EN 12440) by immersion in water at atmospheric pressure. According to the foreword it is one of a series of CEN/TC 246 standards on test methods for natural stone (among others EN 1925 — water absorption coefficient by capillarity, EN 1936 — density and porosity, EN 12371 — frost resistance, EN 12370 — resistance to salt crystallisation); the 2008 edition replaced EN 13755:2001. The standard has no normative references.
ACCORDING TO THE TEXT OF EN 13755:2008 — PRINCIPLE, APPARATUS, SPECIMENS, PROCEDURE, RESULT, TEST REPORT (foreword, clauses 1–9). Principle (clause 3): after drying to constant mass the specimen is weighed and immersed in water at atmospheric pressure for a specified time; water absorption is expressed in per cent from the ratio of the mass of the saturated specimen (at constant mass) to the mass of the dry specimen. Symbols (clause 4): md — mass of the dry specimen [g], mi — successive masses during the test [g], ms — mass of the saturated specimen (after immersion to constant mass) [g], Ab — water absorption at atmospheric pressure [%]. Apparatus (clause 5): flat-bottomed tank with small non-oxidizable and non-absorbent spacers for the specimens; ventilated oven maintaining (70 ± 5) °C; balance accurate to 0,01 g. Specimens (clause 6): sampling is not the responsibility of the laboratory unless requested; at least six specimens from a homogeneous batch; cylinder, cube or prism with a dimension of (70 ± 5) mm or (50 ± 5) mm, cut with a diamond saw or core-drilled; apparent volume from geometric measurements at least 60 ml, ratio of surface to volume from 0,08 mm⁻¹ to 0,20 mm⁻¹ (specimens prepared for compressive or flexural strength tests may be used if they meet this ratio). Drying (6.3): to constant mass at (70 ± 5) °C — constant mass is reached when the difference between two successive weighings at an interval of (24 ± 2) h does not exceed 0,1 % of the first mass; then in a desiccator to room temperature (20 ± 5) °C. Procedure (clause 7): weighing of the dry specimens (md) to the nearest 0,01 g; specimens on spacers in the tank, at least 15 mm from adjacent ones; tap water at (20 ± 10) °C to half the height of the specimens (time t0); at t0 + (60 ± 5) min — to three quarters of the height; at t0 + (120 ± 5) min — complete immersion to a depth of (25 ± 5) mm; at t0 + (48 ± 2) h the specimens are taken out, quickly wiped with a damp cloth and weighed within 1 min to the nearest 0,01 g (mi); then the same every (24 ± 2) h until constant mass (difference between two successive weighings ≤ 0,1 % of the first mass); the last weighing is ms. Result (clause 8): Ab = (ms − md)/md · 100, in per cent to the nearest 0,1 %. Test report (clause 9): among others the number and date of the standard (EN 13755:2008), details of the laboratory and of the client, information from the client (petrographic and commercial name of the stone, country and region of extraction, supplier, direction of the plane of anisotropy marked with two parallel lines, who took the samples, surface finish), dates of delivery, preparation and testing, number and dimensions of the specimens, water absorption of each specimen and the arithmetic mean to the nearest 0,1 %.
STATUS (PKN card as of 13.11.2026). The card for PN-EN 13755:2008 (English version) has no withdrawal label: title "Metody badań kamienia naturalnego -- Oznaczanie nasiąkliwości przy ciśnieniu atmosferycznym", published 25-06-2008, 8 pages, KT 108 for Aggregates and Building Stone, "Implements: EN 13755:2008 [IDT]", "Replaces: PN-EN 13755:2002 - Polish version, PN-EN 13755:2002/AC:2004 - Polish version", ICS 73.020, 91.100.15. In the iTeh catalogue SIST EN 13755:2008 — published.
HOW MANY LABORATORIES AND IN WHAT FORM (accreditation scope database of the service, read 13.11.2026). The notation EN 13755 appears in 6 records at 5 Polish laboratories: "PN-EN 13755:2008" — AB 298, AB 1251 and AB 1344; "PN-EN 13755:2008+AC:2004" — AB 005 (two records: rocks and stone materials, and concrete); "PN-EN 13755" without a date — AB 023. Outside Poland — 3 Czech laboratories (ČSN EN 13755, in 1166.4 alongside ČSN EN 12326-2 and ČSN EN 1097-6).
WHAT THE LABORATORIES TEST (scope database, complete items — 5 Polish). Natural stone — water absorption at atmospheric pressure (AB 1251); compact rocks and stone elements (AB 298); paving setts, kerbs, slabs for external paving, cladding and modular tiles of natural stone — gravimetric method (AB 1344); rocks and stone materials and concrete — water absorption, gravimetric method (AB 005); in AB 023 the record with the standard in the database combines water absorption (0,0–20) % with frost resistance. Concrete (AB 005) is outside the scope of EN 13755, which concerns natural stone.
WHERE AN APPARENTLY CORRECT RESULT IS EASY TO GET. Specimens: fewer than six, dimension outside (70 ± 5) mm or (50 ± 5) mm, volume below 60 ml or surface-to-volume ratio outside 0,08–0,20 mm⁻¹. Drying: temperature higher than (70 ± 5) °C, constant mass without checking the difference ≤ 0,1 % over 24 h, weighing before cooling in the desiccator. Immersion: complete at once instead of in stages (½, after 60 min ¾, after 120 min fully under 25 mm of water), specimens closer than 15 mm to each other, no spacers. Weighing of saturated specimens: wiping too long or weighing later than 1 min after removal; ending after 48 h without reaching constant mass.
WHAT WE DO NOT GIVE. Part read: the iTeh sample of SIST EN 13755:2008 (English version) — foreword and clauses 1–9 in full; the test report requirements (clause 9) are given in abbreviated form. The PKN catalogue returns two cards for this number: PN-EN 13755:2002 (Polish version) and PN-EN 13755:2008 (English version); we did not examine the differences between the 2002 and 2008 editions.
Method principle
At least six stone specimens (cube, cylinder or prism with a dimension of 70 mm or 50 mm) are dried to constant mass at (70 ± 5) °C, cooled in a desiccator and weighed (md). The specimens are immersed in tap water at (20 ± 10) °C in stages — to ½ of the height, after 60 min to ¾, after 120 min completely under 25 mm of water — and after 48 h and then every 24 h wiped with a damp cloth and weighed within 1 min, until the difference between two weighings does not exceed 0,1 % (ms). The water absorption Ab = (ms − md)/md · 100 % is reported to the nearest 0,1 %.
Applications
- Natural stone — water absorption by immersion at atmospheric pressure (EN 13755:2008, clause 1)
- A standard from the series of CEN/TC 246 test methods for natural stone (foreword)
- Specimens for compressive or flexural strength tests — if they meet the surface-to-volume ratio (6.2, note)
- In accreditation scopes: 5 Polish laboratories — natural stone, rocks, stone products for paving and cladding; 3 Czech
Key parameters
| Parameter | Value |
|---|---|
| STATUS (PKN card as of 13.11.2026) | PN-EN 13755:2008 current (English version, published 25-06-2008); implements EN 13755:2008; replaced PN-EN 13755:2002 and AC:2004 |
| Specimens (6.1–6.2) | ≥ 6 from a homogeneous batch; cylinder, cube or prism (70 ± 5) mm or (50 ± 5) mm; ≥ 60 ml; surface/volume 0,08–0,20 mm⁻¹ |
| Drying (6.3) | (70 ± 5) °C to constant mass (difference ≤ 0,1 % at an interval of (24 ± 2) h); cooling in a desiccator to (20 ± 5) °C |
| Immersion (clause 7) | tap water (20 ± 10) °C: t0 — ½ of the height; t0 + (60 ± 5) min — ¾; t0 + (120 ± 5) min — fully under (25 ± 5) mm of water; spacing ≥ 15 mm |
| Weighing (clause 7) | at t0 + (48 ± 2) h, then every (24 ± 2) h; wiping with a damp cloth, weighing within ≤ 1 min to the nearest 0,01 g; to constant mass (≤ 0,1 %) |
| Result (clause 8) | Ab = (ms − md)/md · 100 [%], to the nearest 0,1 %; each specimen and the mean in the report |
| Coverage in accreditation scopes (database, read 13.11.2026) | 5 Polish laboratories, 6 records; 3 Czech |
Standard
- Standard number
- PN-EN 13755:2008 (English version; implements EN 13755:2008 [IDT])
- Title (PL)
- Metody badań kamienia naturalnego — Oznaczanie nasiąkliwości przy ciśnieniu atmosferycznym
- Title (EN)
- Natural stone test methods — Determination of water absorption at atmospheric pressure
Step-by-step procedure
-
Specimens
≥ 6 specimens from a homogeneous batch, 70 mm or 50 mm, ≥ 60 ml, surface/volume 0,08–0,20 mm⁻¹; cutting with a diamond saw or core drilling (6.1–6.2).
-
Drying
(70 ± 5) °C to constant mass (difference ≤ 0,1 % after (24 ± 2) h), cooling in a desiccator to (20 ± 5) °C, weighing md to the nearest 0,01 g (6.3, clause 7).
-
Immersion in stages
On spacers, ≥ 15 mm apart; water (20 ± 10) °C to ½ of the height (t0), after (60 ± 5) min to ¾, after (120 ± 5) min completely under (25 ± 5) mm of water (clause 7).
-
Weighing
At t0 + (48 ± 2) h and then every (24 ± 2) h: removal, quick wiping with a damp cloth, weighing within 1 min (mi) and re-immersion (clause 7).
-
Constant mass and result
Until the difference between two successive weighings ≤ 0,1 %; the last weighing = ms; Ab = (ms − md)/md · 100 to the nearest 0,1 % (clauses 7–8).
-
Test report
Standard, laboratory, client, petrographic and commercial name of the stone, origin, anisotropy, dates, number and dimensions of the specimens, Ab of each specimen and the mean (clause 9).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Flat-bottomed tank (5.1) | With small non-oxidizable and non-absorbent spacers for the specimens | — |
| Ventilated oven (5.2) | Maintains (70 ± 5) °C | — |
| Balance (5.3) | Accuracy 0,01 g | — |
| Desiccator (6.3) | For cooling the dried specimens to (20 ± 5) °C | — |
| Diamond saw or core drill (6.2) | For cutting the specimens | — |
Reagents, media and consumables
| Reagent | CAS | Details |
|---|---|---|
| Tap water (clause 7) | — | At (20 ± 10) °C — for immersing the specimens |
Health and safety (OHS)
- The standard contains no safety warning in the text read; specimens are cut with a diamond saw or core drill (6.2)
- TECHNICAL NOTE: sampling is not the responsibility of the laboratory unless the client requests it (6.1)
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN 13755:2008 (English version; implements EN 13755:2008 [IDT]) — “Natural stone test methods — Determination of water absorption at atmospheric pressure”.
How does this method work?
At least six stone specimens (cube, cylinder or prism with a dimension of 70 mm or 50 mm) are dried to constant mass at (70 ± 5) °C, cooled in a desiccator and weighed (md). The specimens are immersed in tap water at (20 ± 10) °C in stages — to ½ of the height, after 60 min to ¾, after 120 min completely under 25 mm of water — and after 48 h and then every 24 h wiped with a damp cloth and weighed within 1 min, until the difference between two weighings does not exceed 0,1 % (ms).
What is the measuring range and accuracy?
STATUS (PKN card as of 13.11.2026): PN-EN 13755:2008 current (English version, published 25-06-2008); implements EN 13755:2008; replaced PN-EN 13755:2002 and AC:2004; Specimens (6.1–6.2): ≥ 6 from a homogeneous batch; cylinder, cube or prism (70 ± 5) mm or (50 ± 5) mm; ≥ 60 ml; surface/volume 0,08–0,20 mm⁻¹; Drying (6.3): (70 ± 5) °C to constant mass (difference ≤ 0,1 % at an interval of (24 ± 2) h); cooling in a desiccator to (20 ± 5) °C; Immersion (clause 7): tap water (20 ± 10) °C: t0 — ½ of the height; t0 + (60 ± 5) min — ¾; t0 + (120 ± 5) min — fully under (25 ± 5) mm of water; spacing ≥ 15 mm.
How long does the test take?
The times given for the individual stages add up to approximately 2 days 2 h. The procedure comprises 6 steps.
What equipment is required?
Flat-bottomed tank (5.1), Ventilated oven (5.2), Balance (5.3), Desiccator (6.3), Diamond saw or core drill (6.2).
Where is this test used?
Natural stone — water absorption by immersion at atmospheric pressure (EN 13755:2008, clause 1); A standard from the series of CEN/TC 246 test methods for natural stone (foreword); Specimens for compressive or flexural strength tests — if they meet the surface-to-volume ratio (6.2, note); In accreditation scopes: 5 Polish laboratories — natural stone, rocks, stone products for paving and cladding; 3 Czech.
What safety precautions apply?
The standard contains no safety warning in the text read; specimens are cut with a diamond saw or core drill (6.2); TECHNICAL NOTE: sampling is not the responsibility of the laboratory unless the client requests it (6.1).
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN 13755.