🎨 Paints and varnishes — water-vapour transmission through coatings: cup method (wet cup with saturated ammonium dihydrogen phosphate solution — reference method, dry cup with desiccant), water-vapour transmission rate V, water-vapour diffusion-equivalent air layer thickness sd, water-vapour resistance factor μ; PN-EN ISO 7783
In short
Determination of the water-vapour transmission properties of coatings of paints, varnishes and related products, self-supporting and on a porous substrate. The test is performed according to PN-EN ISO 7783:2018-11 (English version; implements EN ISO 7783:2018 and ISO 7783:2018 [IDT]); STATUS (as of 20.11.2026): PKN card: PN-EN ISO 7783:2018-11 “Farby i lakiery -- Oznaczanie właściwości przenikania pary wodnej -- Metoda z zastosowaniem naczynka” — English version (published 27-11-2018, 32 pages), KT 175 Paints and Varnishes, implements EN ISO 7783:2018 and ISO 7783:2018 [IDT], replaces PN-EN ISO 7783:2012 and PN-EN ISO 7783:2012/Ap1:2015-12 (Polish versions); the card gives no withdrawal date. The PKN search for “PN-EN ISO 7783” returns no Polish version of the 2018 edition. At the publisher, ISO 7783:2018 has the status “Published” (iTeh catalogue card). The procedure comprises 4 steps; it is used for: Coatings of paints, varnishes and related products — self-supporting and non-self-supporting on a porous substrate (clause 1, 3.5, 3.6), Coatings for interiors and dry places (conditioning method A) and coatings exposed to rain (method B with soaking and drying cycles) (6.2.3), Tests at high humidity (wet cup, between 93 % and 50 %) and at low humidity (dry cup, between 50 % and 3 %) (3.7, 3.8).
At a glance
- Standard: PN-EN ISO 7783:2018-11 (English version; implements EN ISO 7783:2018 and ISO 7783:2018 [IDT])
- Category: Materials and NDT
- Procedure steps: 4
- STATUS (as of 20.11.2026): PKN card: PN-EN ISO 7783:2018-11 “Farby i lakiery -- Oznaczanie właściwości przenikania pary wodnej -- Metoda z zastosowaniem naczynka” — English version (published 27-11-2018, 32 pages), KT 175 Paints and Varnishes, implements EN ISO 7783:2018 and ISO 7783:2018 [IDT], replaces PN-EN ISO 7783:2012 and PN-EN ISO 7783:2012/Ap1:2015-12 (Polish versions); the card gives no withdrawal date. The PKN search for “PN-EN ISO 7783” returns no Polish version of the 2018 edition. At the publisher, ISO 7783:2018 has the status “Published” (iTeh catalogue card).
- Limit of the scope (clause 1): V above 680 g/(m2⋅d), i.e. sd below 0,03 m — result not accurate
- Wet cup — reference method (5.3): saturated NH4H2PO4 solution, 93 % humidity in the cup, enclosure 50 %, vapour pressure difference 1 207 Pa (23 °C, 101 325 Pa)
Overview
WHAT THE STANDARD COVERS. According to clause 1 of ISO 7783:2018 the standard specifies a method for determining the water-vapour transmission properties of coatings of paints, varnishes and related products. It supplements ISO 12572, from which the procedure, the definitions and the calculations have been taken over as far as possible. Water-vapour transmission rates of more than 680 g/(m2⋅d), i.e. water-vapour diffusion-equivalent air layer thicknesses sd of less than 0,03 m, are not accurately quantified by this method.
ACCORDING TO THE TEXT OF ISO 7783:2018 (second edition; publisher's sample: foreword, introduction, clauses 1–6.2.3). The standard was prepared by ISO/TC 35 (paints and varnishes), subcommittee SC 9 (general test methods for paints and varnishes). The second edition replaces the first (ISO 7783:2011) as a minor revision: the conversion factor in Formula (3) was corrected and a reference to ISO 4618 was added in clause 3. According to the introduction, the transmission rate is not necessarily a linear function of film thickness, temperature or relative-humidity difference, so test conditions are chosen as close as possible to the conditions of use; the wet-cup method is the reference method, and other procedures and conditions, e.g. the dry cup, are used by agreement.
QUANTITIES (clause 3). Water-vapour transmission rate V — mass of water vapour transmitted over a given period through a given surface area of a test piece under specified constant relative humidity at each face, in g/(m2⋅d); measured at pressure p it is converted to standard pressure p0 by multiplying by p/p0, and the factor 20,4 links it with sd. Rate of flow of water vapour through the test piece G — in grams per hour. Water-vapour diffusion-equivalent air layer thickness sd — thickness of a static air layer with the same transmission rate, in metres. Water-vapour resistance factor μ — how many times greater the resistance of the material is than that of an air layer of the same thickness; meaningful only if the transmission rate does not depend on thickness, which is normally not the case for coatings.
PRINCIPLE AND APPARATUS (clauses 4–5). The cup with the test piece is placed in an enclosure at a specified temperature (e.g. 23 °C) and relative humidity (e.g. 50 %). Inside the cup 93 % relative humidity is maintained with a saturated solution of ammonium dihydrogen phosphate NH4H2PO4 with undissolved crystals (wet-cup method, water vapour pressure difference 1 207 Pa at 23 °C and 101 325 Pa) or 3 % with a desiccant — silica gel granules passing a 4 mm sieve and retained on a 1,6 mm sieve, or anhydrous calcium chloride dried at 200 °C (dry-cup method, 1 400 Pa). Substrate for non-self-supporting coatings: homogeneous porous material with a transmission rate above 240 g/(m2⋅d), e.g. polyethylene frits, cellular-concrete discs, glass frits, unglazed ceramic tiles. Cup of glass, plastic or metal; exposed area at least 50 cm2 (non-self-supporting coatings) or 10 cm2 (self-supporting); air gap between test piece and solution or desiccant from 10 mm to 30 mm. Sealing without solvents (mechanical clamps, wax, two-component materials; molten wax — Annex B). Enclosure for the reference method: (23 ± 2) °C and (50 ± 5) % relative humidity according to ISO 3270, air flow over the test piece from 0,02 m/s to 0,3 m/s, conditions re-established not more than 15 min after closing the door. Balance: accuracy 1 mg for test areas up to 50 cm2, 10 mg for larger ones.
PREPARATION (clause 6). Samples of the product are taken according to ISO 15528 and prepared according to ISO 1513. The product is applied to the substrate according to the manufacturer's instructions — not less than the indicated amount and not more than 50 % more; the coating shall be continuous, homogeneous and free from visible imperfections. Self-supporting coatings are made on a substrate from which they detach easily (e.g. glass coated with high-density polyethylene or polytetrafluoroethylene), cut out with a template, and test pieces with pinholes are discarded. Test pieces are dried for 7 days in freely circulating air at (23 ± 2) °C and (50 ± 5) % relative humidity. Conditioning: method A (coatings not exposed to rain) — 28 days at (23 ± 2) °C and (50 ± 5) % or until the mass difference between weighings at 24 h intervals is less than 1 %; method B (coatings exposed to rain) — 3 cycles: 24 h in tap water at (23 ± 2) °C and 24 h drying at (50 ± 2) °C.
WHAT WE DO NOT GIVE HERE. The sample ends at 6.2.3 (conditioning). We do not reproduce the determination of coating thickness (6.3), the preparation of test assemblies (6.4), the weighing procedure (clause 7), the calculation formulae for V, sd and μ (clause 8), the precision data (clause 9) or the content of the test report (clause 10), because they are not in the text we read.
STATUS (as of 20.11.2026). PKN card: PN-EN ISO 7783:2018-11 “Farby i lakiery -- Oznaczanie właściwości przenikania pary wodnej -- Metoda z zastosowaniem naczynka” — English version (published 27-11-2018, 32 pages), KT 175 Paints and Varnishes, implements EN ISO 7783:2018 and ISO 7783:2018 [IDT], replaces PN-EN ISO 7783:2012 and PN-EN ISO 7783:2012/Ap1:2015-12 (Polish versions); the card gives no withdrawal date. The PKN search for “PN-EN ISO 7783” returns no Polish version of the 2018 edition. At the publisher, ISO 7783:2018 has the status “Published” (iTeh catalogue card).
Method principle
A self-supporting coating or a coating on a porous substrate is sealed to the rim of a cup in which 93 % relative humidity is maintained with a saturated ammonium dihydrogen phosphate solution (wet-cup method, reference) or 3 % with a desiccant (dry-cup method), and placed in an enclosure at constant temperature and humidity, e.g. 23 °C and 50 %. Water vapour diffuses through the coating because of the difference in partial pressures; the water-vapour transmission rate and the diffusion-equivalent air layer thickness are calculated from the change in mass of the assembly weighed at intervals and from the test area.
Applications
- Coatings of paints, varnishes and related products — self-supporting and non-self-supporting on a porous substrate (clause 1, 3.5, 3.6)
- Coatings for interiors and dry places (conditioning method A) and coatings exposed to rain (method B with soaking and drying cycles) (6.2.3)
- Tests at high humidity (wet cup, between 93 % and 50 %) and at low humidity (dry cup, between 50 % and 3 %) (3.7, 3.8)
- Determination of the transmission rate V, the diffusion-equivalent air layer thickness sd and the resistance factor μ (clauses 3, 8)
Key parameters
| Parameter | Value |
|---|---|
| STATUS (as of 20.11.2026) | PKN card: PN-EN ISO 7783:2018-11 “Farby i lakiery -- Oznaczanie właściwości przenikania pary wodnej -- Metoda z zastosowaniem naczynka” — English version (published 27-11-2018, 32 pages), KT 175 Paints and Varnishes, implements EN ISO 7783:2018 and ISO 7783:2018 [IDT], replaces PN-EN ISO 7783:2012 and PN-EN ISO 7783:2012/Ap1:2015-12 (Polish versions); the card gives no withdrawal date. The PKN search for “PN-EN ISO 7783” returns no Polish version of the 2018 edition. At the publisher, ISO 7783:2018 has the status “Published” (iTeh catalogue card). |
| Limit of the scope (clause 1) | V above 680 g/(m2⋅d), i.e. sd below 0,03 m — result not accurate |
| Wet cup — reference method (5.3) | saturated NH4H2PO4 solution, 93 % humidity in the cup, enclosure 50 %, vapour pressure difference 1 207 Pa (23 °C, 101 325 Pa) |
| Dry cup (5.4) | silica gel (sieves 4 mm / 1,6 mm) or anhydrous CaCl2 dried at 200 °C, 3 % humidity, difference 1 400 Pa |
| Enclosure (5.6) | (23 ± 2) °C, (50 ± 5) % relative humidity, air flow 0,02–0,3 m/s, conditions restored ≤ 15 min |
| Cup (5.2) | exposed area ≥ 50 cm2 (non-self-supporting coatings) or ≥ 10 cm2 (self-supporting); air gap 10–30 mm |
| Balance (5.7) | accuracy 1 mg (test area up to 50 cm2) or 10 mg (above 50 cm2) |
| Conditioning (6.2.3) | A: 28 days at (23 ± 2) °C and (50 ± 5) % or until mass change < 1 % per 24 h; B: 3 cycles of 24 h in water at (23 ± 2) °C + 24 h at (50 ± 2) °C |
Standard
- Standard number
- PN-EN ISO 7783:2018-11 (English version; implements EN ISO 7783:2018 and ISO 7783:2018 [IDT])
- Title (PL)
- Farby i lakiery — Oznaczanie właściwości przenikania pary wodnej — Metoda z zastosowaniem naczynka
- Title (EN)
- Paints and varnishes — Determination of water-vapour transmission properties — Cup method
Step-by-step procedure
-
Sampling and preparation of the product
Sampling according to ISO 15528, preparation according to ISO 1513 (6.1).
-
Making the test pieces
Coating on a porous substrate (amount from the indicated one up to +50 %) or self-supporting coating detached from the substrate and cut with a template; drying for 7 days at (23 ± 2) °C and (50 ± 5) % (6.2.1, 6.2.2).
-
Conditioning
Method A (28 days or until constant mass) for coatings not exposed to rain or method B (3 soaking and drying cycles) for coatings exposed to rain (6.2.3).
-
Assembly and exposure
Sealing the test piece on a cup with saturated NH4H2PO4 solution or with desiccant, placing it in the enclosure at (23 ± 2) °C and (50 ± 5) %, weighings at intervals (clauses 4, 5).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Test cup (5.2) | Of glass, plastic or metal, resistant to corrosion; for aluminium a wall thickness of 1 mm is sufficient | — |
| Test enclosure (5.6) | Controlled temperature and relative humidity, air flow over the test piece from 0,02 m/s to 0,3 m/s | — |
| Balance (5.7) | Accuracy 1 mg or 10 mg depending on the test area, preferably inside the enclosure | — |
| Porous substrate (5.1) | Polyethylene frits, cellular-concrete discs, glass frits, unglazed ceramic tiles — transmission rate above 240 g/(m2⋅d) | — |
| Cutting template (6.2.2) | Cutting specimens of self-supporting coatings to a size suitable for the cup (Figure B.1) | — |
Reagents, media and consumables
| Reagent | CAS | Details |
|---|---|---|
| Ammonium dihydrogen phosphate NH4H2PO4 (5.3) | — | analytical grade; saturated solution with undissolved crystals, water of at least grade 3 according to ISO 3696 |
| Silica gel (5.4) | — | dried; granules passing a 4 mm sieve, retained on a 1,6 mm sieve |
| Anhydrous calcium chloride (5.4) | — | dried at 200 °C |
| Sealing material (5.5) | — | impermeable, free from cracks, without solvents or volatile constituents (e.g. wax) |
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN ISO 7783:2018-11 (English version; implements EN ISO 7783:2018 and ISO 7783:2018 [IDT]) — “Paints and varnishes — Determination of water-vapour transmission properties — Cup method”.
How does this method work?
A self-supporting coating or a coating on a porous substrate is sealed to the rim of a cup in which 93 % relative humidity is maintained with a saturated ammonium dihydrogen phosphate solution (wet-cup method, reference) or 3 % with a desiccant (dry-cup method), and placed in an enclosure at constant temperature and humidity, e.g.
What is the measuring range and accuracy?
STATUS (as of 20.11.2026): PKN card: PN-EN ISO 7783:2018-11 “Farby i lakiery -- Oznaczanie właściwości przenikania pary wodnej -- Metoda z zastosowaniem naczynka” — English version (published 27-11-2018, 32 pages), KT 175 Paints and Varnishes, implements EN ISO 7783:2018 and ISO 7783:2018 [IDT], replaces PN-EN ISO 7783:2012 and PN-EN ISO 7783:2012/Ap1:2015-12 (Polish versions); the card gives no withdrawal date. The PKN search for “PN-EN ISO 7783” returns no Polish version of the 2018 edition. At the publisher, ISO 7783:2018 has the status “Published” (iTeh catalogue card).; Limit of the scope (clause 1): V above 680 g/(m2⋅d), i.e. sd below 0,03 m — result not accurate; Wet cup — reference method (5.3): saturated NH4H2PO4 solution, 93 % humidity in the cup, enclosure 50 %, vapour pressure difference 1 207 Pa (23 °C, 101 325 Pa); Dry cup (5.4): silica gel (sieves 4 mm / 1,6 mm) or anhydrous CaCl2 dried at 200 °C, 3 % humidity, difference 1 400 Pa.
How long does the test take?
The procedure comprises 4 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.
What equipment is required?
Test cup (5.2), Test enclosure (5.6), Balance (5.7), Porous substrate (5.1), Cutting template (6.2.2).
Where is this test used?
Coatings of paints, varnishes and related products — self-supporting and non-self-supporting on a porous substrate (clause 1, 3.5, 3.6); Coatings for interiors and dry places (conditioning method A) and coatings exposed to rain (method B with soaking and drying cycles) (6.2.3); Tests at high humidity (wet cup, between 93 % and 50 %) and at low humidity (dry cup, between 50 % and 3 %) (3.7, 3.8); Determination of the transmission rate V, the diffusion-equivalent air layer thickness sd and the resistance factor μ (clauses 3, 8).
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 7783.