🔩 Paints and varnishes — cupping test: coated panel clamped between the retaining ring and the drawing die (bore 27 mm), hemispherical indenter of 20 mm diameter pushed from the substrate side at a steady 0,1–0,3 mm/s to a specified depth ("pass/fail" result) or to the first cracking or detachment of the coating (minimum depth, to the nearest 0,1 mm), duplicate determinations at (23 ± 2) °C; PN-EN ISO 1520
In short
An empirical method for assessing the resistance of a coating of paint, varnish or related product to cracking and detachment from a metal substrate under gradual deformation by indentation. The test is performed according to PN-EN ISO 1520:2007 (Polish version; implements EN ISO 1520:2006 and ISO 1520:2006 [IDT]); STATUS (PKN card as of 13.11.2026): PN-EN ISO 1520:2007 current (Polish version, published 25-10-2007); implements EN ISO 1520:2006 and ISO 1520:2006. The procedure comprises 6 steps; it is used for: Coatings of paints, varnishes and related products on metal substrates — resistance to cracking and detachment under indentation (ISO 1520:2006, clause 1), Single coats or the complete multi-coat system (clause 1), "Pass/fail" test to a specified depth or determination of the minimum cracking depth (clauses 1, 7.2–7.3).
At a glance
- Standard: PN-EN ISO 1520:2007 (Polish version; implements EN ISO 1520:2006 and ISO 1520:2006 [IDT])
- Category: Materials and NDT
- Procedure steps: 6
- STATUS (PKN card as of 13.11.2026): PN-EN ISO 1520:2007 current (Polish version, published 25-10-2007); implements EN ISO 1520:2006 and ISO 1520:2006
- Indenter (4.1.3, Fig. 1): hemisphere Ø20 mm (SØ20 ± 0,05), hardened polished steel; deviation from the axis ≤ 0,1 mm; no rotation
- Die and ring (Fig. 1): die bore Ø27 ± 0,05 mm, edge R0,75 ± 0,05 mm; ring bore Ø33 ± 0,1 mm
Overview
WHAT THE STANDARD COVERS. According to clause 1 of ISO 1520:2006 the standard specifies an empirical method for assessing the resistance of a coating of paint, varnish or related product to cracking or detachment from a metal substrate when subjected to gradual deformation by indentation under standard conditions. For a multi-coat system each coat may be tested separately or the complete system. The method is carried out as a "pass/fail" test — to a specified depth of indentation — or by gradually increasing the depth to determine the minimum depth at which the coating cracks or becomes detached from the substrate. According to the introduction it is one of six standards for empirical deformation tests of coatings (alongside ISO 1519, ISO 6272-1, ISO 6272-2, ISO 6860 and ISO 17132); the tests differ technically and in accuracy.
ACCORDING TO THE TEXT OF ISO 1520:2006 — PRINCIPLE, APPARATUS, PANELS, PROCEDURE (foreword, introduction, clauses 1–8). The standard was prepared by ISO/TC 35 (Paints and varnishes), subcommittee SC 9; the third edition replaced ISO 1520:1999 — the determination is carried out in duplicate instead of triplicate, precision data were added. Principle (clause 3): the product is applied at uniform thickness to flat panels of uniform surface texture; after drying the panel is placed between the retaining ring and the drawing die and a hemispherical indenter is pushed into the die at a steady rate, forming a dome with the coating on the outside. Apparatus (4.1, Figure 1): drawing die of surface-hardened steel with a plane-polished contact surface, bore Ø27 ± 0,05 mm with an edge radius of R0,75 ± 0,05 mm; retaining ring with a bore of Ø33 ± 0,1 mm, plane-polished and parallel to the die (outer diameter of both Ø55 ± 0,1 mm); indenter of hardened polished steel ending in a hemisphere of 20 mm diameter (SØ20 ± 0,05) — mechanical drive preferred, hand operation allowed if the conditions of clause 7 are achieved; the indenter shall not turn, the centre of the spherical part shall not deviate from the die axis by more than 0,1 mm, steady speed 0,1–0,3 mm/s; at the zero position the tip of the hemisphere lies in the plane of the ring, touches the panel and is in the centre of the die bore. Measuring devices (4.1.4): depth to the nearest 0,1 mm, panel thickness to 0,01 mm; microscope or magnifier (4.2), preferably up to ×10 magnification. Sampling (clause 5): according to ISO 15528, preparation according to ISO 1513. Panels (clause 6): substrate according to ISO 1514, flat, free from distortion, withstanding the cupping test without cracking (if the substrate cracks before the coating, the coating result can be reported as better than the depth at which the substrate cracked); rectangular, thickness from 0,3 mm to 1,25 mm (measured to the nearest 0,01 mm); two tests on one long strip or on two panels — indentation centres at least 35 mm from any edge and at least 70 mm apart; panels may be cut to size after coating if no distortion occurs; preparation according to ISO 1514; drying (or stoving) and ageing as specified, conditioning for at least 16 h at (23 ± 2) °C and (50 ± 5) % relative humidity; coating thickness according to ISO 2808. Procedure (clause 7): duplicate determinations at (23 ± 2) °C and (50 ± 5) % (ISO 3270). At one specified depth (7.2): the panel is held without excessive pressure between the ring and the die, coating towards the die, the indenter just touching the uncoated side (zero position), the indenter axis at least 35 mm from the edge; the indenter is pushed in at a steady speed to the specified depth; the coating is examined with normal or corrected vision and, if necessary, with a microscope or ×10 magnifier — use of the instrument is stated in the test report. At the minimum depth (7.3): indentation continues until the first crack or the beginning of detachment of the coating, the indenter is stopped and the depth is measured to the nearest 0,1 mm; the result is confirmed on a new panel (if the results differ — additional determinations). Supplementary conditions to be stated (clause 8): material, dimensions and surface preparation of the substrate, method of application, duration and conditions of drying and ageing, dry film thickness with the measuring method and whether it is a single coat, temperature and humidity during the test.
STATUS (PKN card as of 13.11.2026). The card for PN-EN ISO 1520:2007 (Polish version) has no withdrawal label: title "Farby i lakiery -- Badanie tłoczności", published 25-10-2007, 12 pages, KT 175 for Paints and Varnishes, "Implements: EN ISO 1520:2006 [IDT], ISO 1520:2006 [IDT]", "Replaces: PN-EN ISO 1520:2007 - English version, PN-EN ISO 1520:2007 - German version", ICS 87.040. ISO 1520:2006 in the iTeh catalogue — published, stage "International Standard confirmed".
HOW MANY LABORATORIES AND IN WHAT FORM (accreditation scope database of the service, read 13.11.2026). The notation ISO 1520 appears in 5 records at 5 Polish laboratories: "PN-EN ISO 1520:2007" — AB 1424, AB 240 and AB 163 (together with PN-EN ISO 1513:2010); "PN-EN ISO 1520" without a date — AB 369 and AB 023. Outside Poland — 2 Czech laboratories (1322 — ČSN EN ISO 1520; 1125 — Metodika č. 14 based on ČSN EN ISO 1520).
WHAT THE LABORATORIES TEST (scope database, complete items — 5 Polish). Paint systems on metal substrates (AB 1424); paint systems, anticorrosive coatings and coverings (AB 369); organic coatings of paint products and plastics (AB 240); coatings (AB 163); coating products for the protection of metal elements — "slow deformation method", range (0–30) mm (AB 023). All items name the property "cupping resistance".
WHERE AN APPARENTLY CORRECT RESULT IS EASY TO GET. Apparatus: indenter turning or offset from the die axis by more than 0,1 mm, speed outside 0,1–0,3 mm/s, zero position not set in the plane of the ring. Panels: thickness outside 0,3–1,25 mm, indentation centre closer than 35 mm to the edge or 70 mm to the previous one, panel distorted by cutting, conditioning of 16 h omitted. Clamping: excessive pressure of the ring or the coating facing the indenter (the coating has to be on the outside of the dome). Assessment: a result obtained with a magnifier reported like a visual one — the test report has to state the use of the instrument; cracking of the substrate before the coating reported as the coating result.
WHAT WE DO NOT GIVE. Part read: the iTeh sample of ISO 1520:2006 in English (foreword, introduction, clauses 1–7.1, Figure 1) and Russian (clauses 7–8; in the Russian sample the speed in 7.2.3 is written "от 0,1 мм/с до 0,1 мм/с" — we take 0,1–0,3 mm/s from 4.1.3 of the English version). We do not give clause 9 (expression of results), 10 (precision) and 11 (test report) — they are not in the samples. We did not read the Polish text of PN-EN ISO 1520:2007.
Method principle
The product is applied uniformly to a flat metal panel 0,3–1,25 mm thick; after drying and conditioning (≥ 16 h, 23 °C, 50 %) the panel is clamped, coating towards the drawing die (bore Ø27 mm), under the retaining ring. An indenter with a hemispherical end of 20 mm diameter is pushed in from the substrate side at a steady speed of 0,1–0,3 mm/s, forming a dome with the coating on the outside — to a specified depth ("pass/fail" assessment) or until the first cracking or detachment of the coating, when the depth of indentation is measured to the nearest 0,1 mm. The determination is carried out in duplicate.
Applications
- Coatings of paints, varnishes and related products on metal substrates — resistance to cracking and detachment under indentation (ISO 1520:2006, clause 1)
- Single coats or the complete multi-coat system (clause 1)
- "Pass/fail" test to a specified depth or determination of the minimum cracking depth (clauses 1, 7.2–7.3)
- In accreditation scopes: 5 Polish laboratories — paint systems, anticorrosive and organic coatings; 2 Czech
Key parameters
| Parameter | Value |
|---|---|
| STATUS (PKN card as of 13.11.2026) | PN-EN ISO 1520:2007 current (Polish version, published 25-10-2007); implements EN ISO 1520:2006 and ISO 1520:2006 |
| Indenter (4.1.3, Fig. 1) | hemisphere Ø20 mm (SØ20 ± 0,05), hardened polished steel; deviation from the axis ≤ 0,1 mm; no rotation |
| Die and ring (Fig. 1) | die bore Ø27 ± 0,05 mm, edge R0,75 ± 0,05 mm; ring bore Ø33 ± 0,1 mm |
| Indentation speed (4.1.3) | steady, 0,1 mm/s to 0,3 mm/s |
| Measurement (4.1.4) | depth to the nearest 0,1 mm; panel thickness 0,01 mm; magnifier up to ×10 (4.2) |
| Panels (6.2) | thickness 0,3–1,25 mm; indentation centre ≥ 35 mm from the edge, ≥ 70 mm from the second one |
| Conditioning and test (6.4, 7.1) | ≥ 16 h at (23 ± 2) °C and (50 ± 5) % RH; test under the same conditions, duplicate determinations |
| Result (7.3) | minimum depth of indentation at which the coating cracks or detaches — to the nearest 0,1 mm, confirmed on a new panel |
| Coverage in accreditation scopes (database, read 13.11.2026) | 5 Polish laboratories, 5 records; 2 Czech |
Standard
- Standard number
- PN-EN ISO 1520:2007 (Polish version; implements EN ISO 1520:2006 and ISO 1520:2006 [IDT])
- Title (PL)
- Farby i lakiery — Badanie tłoczności
- Title (EN)
- Paints and varnishes — Cupping test
Step-by-step procedure
-
Panels and coating
Substrate according to ISO 1514, flat, 0,3–1,25 mm; application of the product, drying or stoving, conditioning ≥ 16 h at (23 ± 2) °C and (50 ± 5) %; coating thickness according to ISO 2808 (clause 6).
-
Clamping
Panel between the ring and the die without excessive pressure, coating towards the die; indenter at the zero position touching the uncoated side; axis ≥ 35 mm from the edge (7.2.2).
-
Indentation
Steady speed 0,1–0,3 mm/s to the specified depth (7.2) or to the first cracking or detachment of the coating (7.3).
-
Assessment
Examination by eye or with a ×10 magnifier (use of the instrument to be reported); in 7.3 measurement of the depth to the nearest 0,1 mm (7.2.4, 7.3).
-
Repetition
Second determination on a new panel or a second place of the strip (≥ 70 mm from the first); if results differ — additional determinations (7.2.1, 7.3).
-
Data for the report
Substrate, method of application, drying and ageing, dry film thickness with the measuring method, single coat or system, temperature and humidity of the test (clause 8).
Required equipment and apparatus
| Equipment | Example | Indicative price |
|---|---|---|
| Cupping test apparatus (4.1) | Drawing die of surface-hardened steel, retaining ring, indenter with a Ø20 mm hemisphere; mechanical drive preferred, hand operation allowed | — |
| Measuring devices (4.1.4) | Depth of indentation to the nearest 0,1 mm; panel thickness to the nearest 0,01 mm (e.g. micrometer) | — |
| Microscope or magnifier (4.2) | Preferably with magnification up to ×10 — to view the panels during or after deformation | — |
Reagents, media and consumables
| Reagent | CAS | Details |
|---|---|---|
| Not applicable | — | Mechanical test; panels according to ISO 1514, coating thickness according to ISO 2808 |
Health and safety (OHS)
- The standard contains no safety warning in the text read; the apparatus has a moving indenter driven mechanically or by hand (4.1.3)
- TECHNICAL NOTE: if the substrate cracks before the coating, the coating result can be reported as better than the depth at which the substrate cracked (6.1, note)
Frequently asked questions
Which standard describes this test?
The test is performed according to PN-EN ISO 1520:2007 (Polish version; implements EN ISO 1520:2006 and ISO 1520:2006 [IDT]) — “Paints and varnishes — Cupping test”.
How does this method work?
The product is applied uniformly to a flat metal panel 0,3–1,25 mm thick; after drying and conditioning (≥ 16 h, 23 °C, 50 %) the panel is clamped, coating towards the drawing die (bore Ø27 mm), under the retaining ring. An indenter with a hemispherical end of 20 mm diameter is pushed in from the substrate side at a steady speed of 0,1–0,3 mm/s, forming a dome with the coating on the outside — to a specified depth ("pass/fail" assessment) or until the first cracking or detachment of the coating, when the depth of indentation is measured to the nearest 0,1 mm.
What is the measuring range and accuracy?
STATUS (PKN card as of 13.11.2026): PN-EN ISO 1520:2007 current (Polish version, published 25-10-2007); implements EN ISO 1520:2006 and ISO 1520:2006; Indenter (4.1.3, Fig. 1): hemisphere Ø20 mm (SØ20 ± 0,05), hardened polished steel; deviation from the axis ≤ 0,1 mm; no rotation; Die and ring (Fig. 1): die bore Ø27 ± 0,05 mm, edge R0,75 ± 0,05 mm; ring bore Ø33 ± 0,1 mm; Indentation speed (4.1.3): steady, 0,1 mm/s to 0,3 mm/s.
How long does the test take?
The procedure comprises 6 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.
What equipment is required?
Cupping test apparatus (4.1), Measuring devices (4.1.4), Microscope or magnifier (4.2).
Where is this test used?
Coatings of paints, varnishes and related products on metal substrates — resistance to cracking and detachment under indentation (ISO 1520:2006, clause 1); Single coats or the complete multi-coat system (clause 1); "Pass/fail" test to a specified depth or determination of the minimum cracking depth (clauses 1, 7.2–7.3); In accreditation scopes: 5 Polish laboratories — paint systems, anticorrosive and organic coatings; 2 Czech.
What safety precautions apply?
The standard contains no safety warning in the text read; the apparatus has a moving indenter driven mechanically or by hand (4.1.3); TECHNICAL NOTE: if the substrate cracks before the coating, the coating result can be reported as better than the depth at which the substrate cracked (6.1, note).
Which laboratory can perform this test?
The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 1520.