🔩 Ring flexibility of thermoplastics pipes with a circular cross-section — three ring test pieces as in PN-EN ISO 9969 deflected diametrically at a constant speed to a deflection of 30 % of the outside diameter (unless the product standard specifies otherwise), force/deflection graph and checks for cracking, crazing, wall delamination and permanent buckling; PN-EN ISO 13968

Materials and NDT PN-EN ISO 13968

In short

The ring flexibility of a thermoplastics pipe is tested by deflecting diametrically at a constant speed three rings cut from one pipe (as for ring stiffness according to PN-EN ISO 9969) up to the deflection given in the product standard — by default 30 % of the outside diameter — or until earlier failure. The test is performed according to PN-EN ISO 13968:2009 (Polish version; implements EN ISO 13968:2008 and ISO 13968:2008 [IDT]); STATUS (as of 23.11.2026): PKN card: PN-EN ISO 13968:2009 — Polish version, published 10-09-2009, 9 pages, KT 140, implements EN ISO 13968:2008 [IDT] and ISO 13968:2008 [IDT], replaces PN-EN ISO 13968:2008 (English version); the card gives no withdrawal date. The procedure comprises 5 steps; it is used for: Thermoplastics pipes with a circular cross-section, including structured-wall pipes (clause 1, 8.2 c–d), Test required by product standards for drainage and sewerage pipes, which give the deflection and requirements for the force/deflection graph (clause 4, 8.1, bibliography: EN 13476-1), Determination of force and deflection at the first damage or at the maximum force (clause 1, clause 9 f).

At a glance

  • Standard: PN-EN ISO 13968:2009 (Polish version; implements EN ISO 13968:2008 and ISO 13968:2008 [IDT])
  • Category: Materials and NDT
  • Procedure steps: 5
  • STATUS (as of 23.11.2026): PKN card: PN-EN ISO 13968:2009 — Polish version, published 10-09-2009, 9 pages, KT 140, implements EN ISO 13968:2008 [IDT] and ISO 13968:2008 [IDT], replaces PN-EN ISO 13968:2008 (English version); the card gives no withdrawal date.
  • Deflection (8.1): 30 % of the outside diameter unless the referring standard specifies otherwise; change in inside or outside diameter
  • Test pieces (clause 6): three from a single pipe, prepared as in ISO 9969, designated a, b, c; the referring standard may require longer ones

Overview

WHAT THE STANDARD COVERS. According to clause 1 of ISO 13968:2008 the standard specifies a method for testing the ring flexibility of a thermoplastics pipe with a circular cross-section; the method enables determination of the deflection and the necessary force at which physical damage, if any, occurs within the specified diametric deflection. Ring flexibility is, according to 3.1 (after EN 13476-1:2007), the ability of a pipe to resist ring diametric deflection without loss of structural integrity.

ACCORDING TO THE TEXT OF ISO 13968:2008 (edition 2, replacing ISO 13968:1997 after a technical revision; the publisher's sample covers the foreword, clauses 1–9 and the bibliography, i.e. the entire content of the standard). The standard was prepared by committee ISO/TC 138. The apparatus, test pieces, conditioning and compression procedure are taken over from ISO 9969 (ring stiffness) — described in the Knowledge Base in the entry on the ring stiffness of thermoplastics pipes according to PN-EN ISO 9969.

PRINCIPLE (clause 4). A ring section cut from the pipe is deflected diametrically at a constant speed while the force and the deflection are measured, until at least the specified deflection is reached or earlier fracture occurs. Each test piece is monitored during testing and then inspected for several specific types of mechanical failure. The referring standard sets, where appropriate, a greater length of the test pieces than in ISO 9969 and the deflection.

APPARATUS AND TEST PIECES (clauses 5–7). Compression testing machine as in ISO 9969, capable of producing at least the specified diametric deflection of the test piece at the applicable speed (ISO 9969:2007, Table 1); dimensional and force measuring devices conforming to ISO 9969, measuring deflections up to at least the specified one and the corresponding compressive forces. Three test pieces from a single pipe prepared as in ISO 9969, designated a, b and c; the referring standard may require longer test pieces. Conditioning — as in ISO 9969.

PROCEDURE (8.1). The test is carried out according to the procedure of ISO 9969, but compression is continued, measuring the change in inside or outside diameter, until the specified deflection is reached. Unless the referring standard specifies otherwise, the deflection is 30 % of the outside diameter. During compression, signs of failure are monitored until either the deflection is reached or the test piece has failed — whichever occurs first; if desired, compression may be continued to determine other properties of the pipe.

ASSESSMENT (8.2). For each test piece a force/deflection graph is prepared and the type and position of each event are recorded with the corresponding force and deflection: a) compliance of the graph with the requirements of the referring standard; b) cracking or crazing in any part of the wall; c) wall delamination; d) permanent buckling in any part of the wall; e) other observations required by the referring standard. Whitening of the pipe is not considered an indication of any of these failures.

TEST REPORT (clause 9). It includes, among other things, the identification of the pipe (manufacturer, type, dimensions, production date, lengths of test pieces, mass per metre of pipe), the test temperature, the force/deflection graph of each test piece, the force and deflection at the events of 8.2 and the force and deflection at the maximum point, if a maximum occurred.

WHERE A SEEMINGLY CORRECT RESULT IS EASY TO GET. The default deflection refers to the OUTSIDE diameter (30 %), although the change in diameter may be measured inside or outside; whitening is not failure, but cracking, delamination or permanent buckling must be recorded with the force and deflection at which they appeared — a bare result “the test piece reached 30 %” without the graph and inspection of the wall does not meet 8.2.

WHAT WE DO NOT GIVE HERE. We do not repeat the compression speed, test piece length and conditioning of ISO 9969 in this entry — they are in the entry on PN-EN ISO 9969; the standard gives no acceptance criteria (permissible events at a given deflection) — they are set by the product standard.

STATUS (as of 23.11.2026). PKN card: PN-EN ISO 13968:2009 “Systemy przewodów rurowych i rur osłonowych z tworzyw sztucznych -- Rury z tworzyw termoplastycznych -- Oznaczanie elastyczności obwodowej” — Polish version, published 10-09-2009, 9 pages, KT 140 (plastics pipes, fittings and valves), implements EN ISO 13968:2008 [IDT] and ISO 13968:2008 [IDT], replaces PN-EN ISO 13968:2008 (English version); the card gives no withdrawal date.

Method principle

A pipe ring is deflected diametrically at a constant speed to a specified deflection (by default 30 % of the outside diameter) while force and deflection are recorded, and it is checked whether, and at what deflection, cracking, delamination or permanent buckling of the wall occurs.

Applications

Key parameters

ParameterValue
STATUS (as of 23.11.2026)PKN card: PN-EN ISO 13968:2009 — Polish version, published 10-09-2009, 9 pages, KT 140, implements EN ISO 13968:2008 [IDT] and ISO 13968:2008 [IDT], replaces PN-EN ISO 13968:2008 (English version); the card gives no withdrawal date.
Deflection (8.1)30 % of the outside diameter unless the referring standard specifies otherwise; change in inside or outside diameter
Test pieces (clause 6)three from a single pipe, prepared as in ISO 9969, designated a, b, c; the referring standard may require longer ones
Apparatus (5.1, 5.2)compression machine and measuring devices as in ISO 9969, capable of the specified deflection at the speed from ISO 9969:2007, Table 1
Events recorded (8.2)compliance of the force/deflection graph with the product standard; cracking and crazing; wall delamination; permanent buckling; other observations from the product standard
Whitening (8.2)not an indication of mechanical failure
End of compression (8.1)when the deflection is reached or the test piece has failed — whichever occurs first; further compression allowed to determine other properties

Standard

Standard number
PN-EN ISO 13968:2009 (Polish version; implements EN ISO 13968:2008 and ISO 13968:2008 [IDT])
Title (PL)
Systemy przewodów rurowych i rur osłonowych z tworzyw sztucznych — Rury z tworzyw termoplastycznych — Oznaczanie elastyczności obwodowej
Title (EN)
Plastics piping and ducting systems — Thermoplastics pipes — Determination of ring flexibility

Step-by-step procedure

  1. Test pieces

    Three rings from a single pipe as in ISO 9969 (a, b, c); longer if required by the product standard (clause 6).

  2. Conditioning

    As in ISO 9969 (clause 7).

  3. Compression

    Procedure of ISO 9969, continued to the specified deflection — by default 30 % of the outside diameter — measuring the change in inside or outside diameter (8.1).

  4. Monitoring

    During compression, check for signs of failure until the deflection is reached or the test piece fails (8.1).

  5. Assessment and report

    Force/deflection graph for each test piece; record of type, position, force and deflection of each event a)–e); whitening is disregarded (8.2, clause 9).

Required equipment and apparatus

EquipmentExampleIndicative price
Compression testing machine (5.1)As in ISO 9969, capable of producing at least the specified diametric deflection at the speed from ISO 9969:2007, Table 1—
Dimensional and force measuring devices (5.2)Conforming to ISO 9969, measuring deflection up to at least the specified one and the corresponding forces—

Frequently asked questions

Which standard describes this test?

The test is performed according to PN-EN ISO 13968:2009 (Polish version; implements EN ISO 13968:2008 and ISO 13968:2008 [IDT]) — “Plastics piping and ducting systems — Thermoplastics pipes — Determination of ring flexibility”.

How does this method work?

A pipe ring is deflected diametrically at a constant speed to a specified deflection (by default 30 % of the outside diameter) while force and deflection are recorded, and it is checked whether, and at what deflection, cracking, delamination or permanent buckling of the wall occurs.

What is the measuring range and accuracy?

STATUS (as of 23.11.2026): PKN card: PN-EN ISO 13968:2009 — Polish version, published 10-09-2009, 9 pages, KT 140, implements EN ISO 13968:2008 [IDT] and ISO 13968:2008 [IDT], replaces PN-EN ISO 13968:2008 (English version); the card gives no withdrawal date.; Deflection (8.1): 30 % of the outside diameter unless the referring standard specifies otherwise; change in inside or outside diameter; Test pieces (clause 6): three from a single pipe, prepared as in ISO 9969, designated a, b, c; the referring standard may require longer ones; Apparatus (5.1, 5.2): compression machine and measuring devices as in ISO 9969, capable of the specified deflection at the speed from ISO 9969:2007, Table 1.

How long does the test take?

The procedure comprises 5 steps. The standard does not give a duration for every stage — the laboratory's own procedure decides.

What equipment is required?

Compression testing machine (5.1), Dimensional and force measuring devices (5.2).

Where is this test used?

Thermoplastics pipes with a circular cross-section, including structured-wall pipes (clause 1, 8.2 c–d); Test required by product standards for drainage and sewerage pipes, which give the deflection and requirements for the force/deflection graph (clause 4, 8.1, bibliography: EN 13476-1); Determination of force and deflection at the first damage or at the maximum force (clause 1, clause 9 f).

Which laboratory can perform this test?

The test is performed by laboratories accredited to ISO/IEC 17025. On LabCoda you can find them by the standard number PN-EN ISO 13968.